Policy Replication

PHMSA R and D Guidelines for the Identification of SCC Sites and the Estimation of Re-inspection Intervals for SCCDA

Docket document2023-09-20 · PHMSA · report · PHMSA-2011-0023-0757
RIN 2137-AE72, RIN 2137-AF39, RIN 2137-AF38 · Docket PHMSA-2011-0023

Other documents for the same rulemaking

2011-08-25 Federal RegisterPipeline Safety: Safety of Gas Transmission Pipelines
2011-09-19 Docket documentThe Interstate Natural Gas Association of America and the American Gas Association - Request
2011-09-28 Docket documentTexas Pipeline Association - Request for Extension
2011-09-28 Docket documentInterstate Natural Gas Association of America's & American Gas Association's
2011-11-16 Federal RegisterPipeline Safety: Safety of Gas Transmission Pipelines
2011-12-27 Docket documentInterstate Natural Gas Association of America - Letter
2012-01-31 Docket documentStephen and Tina Henning - Comments
2012-02-10 Docket documentINGAA ANPRM Safety of Gas Transmission Pipelines Webinar
2012-10-10 Docket documentU.S. DOT/PHMSA - Meeting with PHMSA and INGAA to discuss comments on Pipeline Safety: Safety of Gas Transmission Pipelines
2012-11-02 Docket documentAmerican Petroleum Institute - Comment
2016-04-07 Docket documentSupporting Document forGas Transmission for NPRM
2016-04-08 Federal RegisterPipeline Safety: Safety of Gas Transmission and Gathering Pipelines
2016-04-11 Docket documentNational Association of Pipeline Safety Representatives Request for Extension- NAPSR 4-8-2016 Sub
2016-04-19 Docket documentCONSOL Energy Inc. Letter - Extension Request U.S DOT PipelineSafety 04192016
2016-05-03 Docket documentSouthwest Gas Corporation - Request for Extension of Comment Period
2016-05-03 Docket documentPennsylvania Public Utility Commission - Request for Extension of Comment Period
2016-05-10 Docket documentAGA, INGAA, API, IPAA, GPA, and APGA- Request for Extension of Comment Period
2016-05-10 Docket documentNew York State of Opportunity Department of Public Service - Extenson of Time Request
2016-05-10 Docket documentMarcellus Shale Coalitition - Extension Request
2016-05-13 Federal RegisterPipeline Safety: Safety of Gas Transmission and Gathering Pipelines
2016-06-09 Docket documentU.S. DOT/PHMSA - Report to Congress - Evaluation of Expanding Pipeline Integrity Management Beyond High-Consequence Areas and Whether Such Expansion Would Mitigate the Need for Gas Pipeline Class Location Requirements - Pipeline Safety, Regulatory Certainty, And Job Creation Act 2011, Section 5
2016-06-27 Docket documentNAPSR - 2016 GasTrans NPRM Extension Request Ltr NAPSR 6-21-2016 Submitted
2016-07-12 Docket documentSafety of Gas Trans Appendix
2016-07-26 Docket documentU.S DOT/PHMSA - Comments of Peoples Natural Gas Company, LLC
2017-03-24 Docket documentU.S. DOT/PHMSA - Notes from Meeting with Pennsylvania Grade Crude Oil Coalition
2017-04-21 Docket documentThe Interstate Natural Gas Association of America (INGAA) - Report - Analysis of Natural Gas Transmission Pipeline Releases and Mitigation Options for Pipeline MAOP Reconfirmation
2017-12-01 Docket documentGas Pipeline Advisory Committee Meeting
2017-12-01 Docket documentGas Pipeline Advisory Committee Meeting Pre-briefing on December 5
2018-03-08 Docket documentU.S. DOT/NHTSA - Final Report - 2017 Mitsubishi Outlander
2018-03-19 Docket documentU.S. DOT/PHMSA - Gas Pipeline Advisory Committee Meeting
2018-04-16 Docket documentGPAC-Slide Presentation Gas Rule - March 26 to 28 Mtg #5-FINAL
2018-12-26 Docket documentGPAC- Gas Gathering Pre-brief presentation
2018-12-26 Docket documentPipeline Safety: Safety of Gas Transmission Pipelines
2019-02-15 Docket documentU.S. DOT/PHMSA - Letters - November 15, 2018, October 10, 2018, Meeting of PHMSA Personnel with Representatives of the Gathering Line Industry
2019-07-16 Docket documentGas Pipeline Advisory Committee Meeting Pre-brief June 19, 2019
2019-07-16 Docket documentGPAC Approved Gas Gathering Lines Vote Slides for June 25-26, 2019 Meeting
2019-07-16 Docket documentGas Pipeline Advisory Committee Meeting Slides for June 25-26, 2019
2019-10-01 Federal RegisterPipeline Safety: Safety of Gas Transmission Pipelines: MAOP Reconfirmation, Expansion of Assessment Requirements, and Other Related Amendments
2019-10-02 Regulatory impact analysisGas Transmission Regulatory Impact Analysis
2019-10-02 Docket documentSubstantive Differences Between the Final Rule Submitted to OIRA on May 21, 2019, and Published in the Federal Register on October 1, 2019, pursuant to EO 12866 Sec. 6(a)(3)(E)
2019-10-02 Docket documentFinal Regulatory Flexibility Act (RFA) Small Business
2019-10-02 Docket documentGas Transmission Final Environmental Assessment
2019-10-24 Docket documentGT Final Rule - GT GG Annual Report and Instructions
2019-10-24 Docket documentGT Final Rule - GT GG Incident Report and Instructions
2019-11-19 Docket documentSummary of Meeting with GPA Midstream on March 29, 2019
2020-03-10 Docket documentAPI Petition Grant Response Letter
2020-03-10 Docket documentAPGA Petition Grant Response Lette
2020-03-10 Docket documentAPGA Petition Grant Response Letter
2020-03-10 Docket documentAGA Petition Grant Response Letter
2020-07-06 Federal RegisterPipeline Safety: Safety of Gas Transmission Pipelines: MAOP Reconfirmation, Expansion of Assessment Requirements, and Other Related Amendments: Response to a Joint Petition for Reconsideration
2021-03-13 Docket documentMeeting with PST dated 2-11-21
2021-10-13 Docket documentEO12866 Meeting - Gas Gathering - API - 10.4.21
2021-10-13 Docket documentEO12866 Meeting Summary - Gas Gathering - GPA 10.5.21
2021-11-12 Docket documentNational Registry Notification Instructions - PHMSA F1000.2 (rev 1-2020) Clean 2021-07-29
2021-11-12 Docket documentGas Gathering Final Rule- Substantive Changes from EO12866 Review
2021-11-12 Docket documentEA Safety of Gas Gathering Pipelines Final Rule
2021-11-12 Docket documentAFPA Briefing to PHMSA 7-16-19
2021-11-14 Regulatory impact analysisFinal RIA/RFA: Safety of Gas Gathering Pipelines
2021-11-14 Docket documentFinal Gas Gathering Forms - Redlines
2021-11-14 Docket documentFinal Gas Gathering Forms and Instructions - Clean

References: 259 extracted, 0 linked to papers

Page 5Download these results: CSV · JSON
Zhang, X.Y., S.B. Lambert, R. Sutherby, and A. Plumtree. 1999. Transgranular stress corrosion cracking of X-60 pipeline steel in simulated ground water. Corrosion 55(3), 297-305.
research reportNot linked to a paper · refsec
Zheng, W., R.W. Revie, F.A. MacLeod, D. Kiff, and S. Rajan. 1995. Testing methods for lowpH pipeline SCC: a comparison of SSRT and full-scale testing. Proc. CORROSION/95,
research reportNot linked to a paper · refsec
Zheng, W., R.W. Revie, O. Dinardo, F.A. MacLeod, W.R. Tyson, and D. Kiff. 1996. Pipeline
research reportNot linked to a paper · refsec
SCC in near-neutral pH environment: effects of environmental and metallurgical variables. Proc. 9th Linepipe Symposium, Pipeline Research Council International, Catalog No. L51746, paper 22. - A-242 Zheng, W., R.W. Revie, W.R. Tyson, G. Shen, F.A. MacLeod, and D. Kiff. 1996. Pipeline SCC in near-neutral pH environment: results of full-scale tests. Proc. CORROSION/96,
research reportNot linked to a paper · refsec
Zheng, W., F.A. MacLeod, R.W. Revie, W.R. Tyson, G. Shen, D. Kiff, M. Skaff, and E-W. Wong. 1997. Recent progress in the study of transgranular SCC in line pipe steels. Proc. 2nd International Conference on Corrosion-Deformation Interactions-CDI '96 (European Federation of Corrosion Report No. 21), paper 28, pp. 282-292.
research reportNot linked to a paper · refsec
Zheng, W., R.W. Revie, F.A. MacLeod, O. Dinardo, D. Kiff, andJ. McKinnon. 1998. Low pH
research reportNot linked to a paper · refsec
Zheng, W., R. Sutherby, R.W. Revie, W.R. Tyson, and G. Shen. 2000. Stress corrosion cracking of linepipe steels in near-neutral pH environment: a review of the effects of stress. In ASTM Special Technical Publication, STP 1401, Environmentally Assisted Cracking Predictive Methods for Risk Assessment and Evaluation of Materials, Equipment and Structures, R.D. Kane (ed.), American Society for Testing and Materials (West Conshohocken, PA), pp. 473-483.
research reportNot linked to a paper · refsec
Zhigletsova, S.K., V.B. Rodin, V.V. Rudavin, G.E. Rasulova, N.A. Alexandrova, G.M. Polomina, and V.P. Kholodenko. 2008. Change of physiochemical parameters of soils near stress-corrosion defects on gas pipelines. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H. Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 323333. - B-1 -
research reportNot linked to a paper · refsec
IGSCC observed in pure sulphate solutions at pH 8 Yunovich et al. (1998)
research reportNot linked to a paper · refsec
IGSCC observed at (cathodic) potentials at which dissolution could not be involved. Contrary to suggestions of a dissolution mechanism for IG cracking Crack path seems dependent on pH with IGSCC prevalent at higher pH. Possible evidence for a transition in crack path from TG to IG with increasing pH. Increasing temperature results in higher crack growth rates and a wider potential window for cracking. The activation energy for high-pH SCC cracks is of the order of 42 kJ/mol. Application of CP current density ca polarize a mill-scaled or rusted steel surface into the cracking range. In lab tests, a cathodic current density of 60 µA/cm2 was sufficient to polarize the surface into the cracking range. iR drop along the disbondment can shift the potential into the cracking range. Thus, the complete loss of CP may not be necessary to shift the potential into the cracking range. The required environment could be generated by CP elsewhere in the disbondment and diffuse to the location of permissible potential. Associated SCC Guideline Yunovich et al. (1998) Yunovich et al. (1998) SzklarskaSmialowska et al. (1994) SzklarskaSmialowska et al. (1994) SzklarskaSmialowska et al. (1994)
research reportNot linked to a paper · refsec
H-0-6 Parkins (1996) H-0-2, H-I-1, H-IV-2 Parkins (1996) H-I-4, H-I-15 Parkins (1996) H-I-4 continued ….. - B-3 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no. H010 H011 H012 H013 H014 H015 R&D Guideline Overprotection at potentials more negative than -1.1 VSCE can result in H2 bubbles that block CP and shift potential into cracking range. Another mechanism by
datasetNot linked to a paper · refsec
SCC failures have been observed for steels with a wide range of chemical composition. Reference Associated SCC Guideline Jack et al. (2000) H-I-2 Sutherby and Chen (2004) Sutherby and Chen (2004) Odziemkowski et al. (1994)
research reportNot linked to a paper · refsec
H-I-7 Parkins (1994) H-I-13 continued ….. - B-6 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no. H029 H030 H031 H032 H033 H034 H035 H036 R&D Guideline Lifetime prediction requires a stochastic approach. Scatter observed in coating failure, crack initiation (which is associated with pitting), crack growth, resulting in a distribution of apparent crack growth rates, which must be treated statistically. High-pH SCC is uncommon on liquid pipelines. Because of the lower temperature generally associated with liquid lines, although there have been vases in warm climates (Saudi Arabia), and the shipment of hot liquids could induce this form of cracking. High-pH SCC cracks follow an intergranular path. This implies a fundamental weakness at grain boundaries, thought to be associated with the cyclic stress-strain behaviour. Field evidence for Fe3O4 with some FeCO3 on fracture surfaces. These observations are consistent with lab findings (see H025) No evidence for role of stress raisers for high-pH SCC. Unlike NNpH SCC for which stress raisers are very important, there is no indication that stress raisers are necessary for high-pH SCC, although cracking has been observed in dents. Probably appropriate to state that stress raisers are not
datasetNot linked to a paper · refsec
H-III-4 H-II-5 H-II-2 Parkins (1994)
research reportNot linked to a paper · refsec
IGSCC is observed over a wide range of pH (pH 6.6-11). Why is high-pH SCC only reported in the range ~pH 9.5-11.5? Is the potential never in the right region? Peak crack growth rate shifts to more-negative potentials with increasing T. On the assumption that more-negative potentials are more likely because of the effects of CP, then high-pH is more likely at higher T. Francis and Jandu (2006)
research reportNot linked to a paper · refsec
H-III-3 Parkins (1996) H-0-5 Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) Parkins and Zhou (1997a) Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) H-IV-2 continued ….. - B-18 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no. H141 H142 H143 H144 H145 H146 H147 H148 H149 H150 R&D Guideline
datasetNot linked to a paper · refsec
SCC crack patterns observed, including the effect of coalescence. Implies no role for effects due to dissolution of inclusions, development of local chemistry, electrochemical effects of millscale, … Once dormant, cracks in a dense patch will remain dormant. I.e., a dense crack patch cannot become a sparse dense patch! Reference Associated SCC Guideline Parkins and Zhou (1997a) H-IV-4 Parkins and Zhou (1997b) Parkins and Zhou (1997b) H-0-6 Parkins and Zhou (1997b)
research reportNot linked to a paper · refsec
Leis (1997) H-III-3 continued ….. - B-19 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no. H151 H152 H153 H154 H155 H156 H157 H158 H159 H160 H161 R&D Guideline Microstructure has effect on crack path. Cracks propagate according to microstructure, tending to prefer propagating along gb, especially in coarsergrained material. Weld metal is less susceptible to high-pH SCC than base metal. Thought to be due to finer grain structure of weld metal. Cracks avoid pearlite or pearlite-dispersed regions. Consistent with suggestion elsewhere that cracks could arrest at pearlite grain boundaries. Mild cyclic loading (R = 0.9) enhances crack initiation by reducing threshold stress. Reported by others, but confirmed here for low stress range Threshold stress lower on as-received (millscale) surface. Although the magnitude of the difference here was not great. Density of cracks increases with increasing load. Implication is that more cracks likely with higher loads, but that the cracks will be denser (and,
government reportNot linked to a paper · refsec
SCC and readily permeates in C-steel and can be concentrated by residual and applied stress is consistent with a role of H in NNpH SCC. Reference Associated SCC Guideline Gu et al. (1999) N-0-7 Gu et al. (1999) N-0-7 Gu et al. (1999) Been et al. (2006) N-I-9, N-IV-1 Been et al. (2006) N-I-9, N-IV-1 Been et al. (2006) N-I-10, N-IV-1, N-IV-2 Qiao and Mao (1998) Qiao et al. (1997)
research reportNot linked to a paper · refsec
N-III-1 Parkins (1998) N-0-9 continued …. - B-26 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N014 N015 N016 N017 N018 N019 N020 R&D Guideline Susceptibility to SCC increases in the presence of CO2. %RA tends to decrease with increasing CO2, although much scatter. At pH 5.8, %RA decreases monotonically with decreasing pH, but at pH 6.5 and pH 8 minimum ductility at around ECORR with second loss of ductility at more-negative potentials (possibly associated with HIC). Proposed role of CO2 is to lower pH to promote H evolution. No systematic effect of temperature. No systematic dependence of %RA on temperature between 5oC and 45oC. Evidence for role of H in NNpH SCC. Cracking occurs at potentials below H equilibrium line, presence of quasi-cleavage on fracture surface characteristic of
datasetNot linked to a paper · refsec
HIC, rather than NNpH SCC, is the predominant process for cathodically polarized samples. Similar %RA at -1.0 VSCE regardless of presence of CO2 or not Rebak et al. (1996) Associated SCC Guideline Brousseau and Qian (1994) Asher and Singh (2009) N-II-6 Asher and Singh (2009) N-II-1 Asher and Singh (2009) N-0-9 Been et al. (2006) N-0-10, N-IV-2, N-IV-4 Been et al. (2006) Gu et al. (1999) N-0-4 Gu et al. (1999) Gu et al. (1999) N-0-7 continued …. - B-29 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N042 N043 N044 N045 N046 N047 N048 N049 R&D Guideline Threshold S content of 0.01-0.02 wt.% for the susceptibility of reactor pressure vessel steels to corrosion fatigue. Similarities between this system and NNpH SCC of pipeline steels proposed by Gabetta (1997). Eadie et al. (2005) proposed important role of S in NNpH SCC environments. Question is whether a similar threshold value exists for NNpH SCC. Hydrogen threshold for HSC/HIC is 10 ppb. If correct, then many of the NNpH SCC studies based on a correlation between H content may, in fact, be related to HSC rather than NNpH SCC. There should exist a potential threshold between NNpH SCC and HSC/HIC. And that threshold, the source of which is a threshold H content, will depend on the nature of the environment (e.g., pH, presence of H-recombination poisons, etc.) Corrosion fatigue mechanism under severe loading conditions. da/dN = C(K)m, for R = 0.5 and 0.82 at 40 cycles/day and R = 0.9 at 5000 cycles/day
datasetNot linked to a paper · refsec
TG cracking. Reference Associated SCC Guideline Beavers and Jaske (2004) N-0-10, N-III-4, N-III-5, N-IV-4 Beavers and Jaske (2004) N-0-10, N-III-4, N-III-5, N-IV-4 Beavers and Jaske (2004) Beavers and Jaske (2004) Beavers and Jaske (2004) N-0-10, N-IV-3 Beavers and Jaske (2004) N-0-10, N-IV-2, N-IV-4 Gangloff (1985)
research reportNot linked to a paper · refsec
N-III-6 Gangloff (1985) continued …. - B-39 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N110 N112 N113 N114 N115 N116 N117 N118 R&D Guideline Environmental enhancement due to effects of cyclic loading on crack chemistry and promotion of H absorption for short cracks. Short cracks have high surface area:volume ratios. O2 consumed on crack walls so that crack-tip pH is maintained low and promotes H+ reduction and H absorption. In the case of HSS, acidification due to hydrolysis of Cr(III). Short cracks grow up to a factor of 10 faster than long cracks in sour environments. Results for X-65 pipeline steel and, although a sour environment, of some relevance to NNpH SCC. At a K~9 MPam1/2, transition from short to long cracks occurs at ~6 mm. Accelerated growth of short cracks likely due to environmental effect on H absorption at crack tip. Could be result of lower crack-tip pH for short cracks or, if bulk charging is most important, gradient of [H] across wall thickness. Crack initiation favoured on original pipe surface and at pits or regions of corrosion. Although original pipe surface was not compared with polished surface, more cracks initiated on external vs. internal surface. Cyclic load tests done under
datasetNot linked to a paper · refsec
CGR. Although the cathodic polarization was done ostensibly to simulate the apparent effect of millscale, could simulate any source of cathodic polarization, e.g., partial CP penetration. Dormant cracks can be reactivated by resumption of more-aggressive cyclic loading. Apparent that dormant cracks are just that, they are dormant rather than dead. Apparently relatively easy to reactivate cracks after as long as 4 days without growth. Crack growth is strongly dependent on strain rate. da/dN decreases but da/dt increases with increasing frequency. Reference Associated SCC Guideline He et al. (2000) Eadie et al. (2002) N-I-9 Eadie et al. (2002) Been et al. (2004) N-I-9 Been et al. (2004) N-I-9, N-II-1 Been et al. (2006) N-0-3 Been et al. (2006) N-I-18 Been et al. (2006) N-III-9 Been et al. (2006) N-0-3 continued …. - B-44 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N156 N157 N158 N159 N160 N161 N162 N163 N164 N165 R&D Guideline NNpH SCC crack growth controlling process changes as crack grows. Threeregime "map' developed, with strain-rate control under mild loading conditions, CF model at intermediate loading conditions, and rapid cracking at high KMAX Under mild loading conditions, a crack-tip strain rate model is appropriate. Based on poor fit of CF model to field data at low KMAX/K, strain rate model deemed to be more appropriate, especially given observation of strain rate dependence of da/dt (da/dt = 0.0085
datasetNot linked to a paper · refsec
CGR is correlated with crack-tip strain rate. However, because of variability in models used to predict , cannot use this correlation to predict CGR's on pipelines. Use frequency and R ratio to rank tendency for cracks to become dormant. Can be done based on correlation in guideline N100, but this figure may be specific to crack geometry and the environment. See also N166 Unload-reload transients can increase the CGR and re-initiate dormant cracks. Occurred in majority of lab cases. Overloads had no consistent effect on CGR or dormant cracks. Neither the occurrence nor the magnitude of overloads had a clear effect in the lab. Simulated hydrotests did not affect dormant cracks but slowed active cracks. Hydrotesting does not re-activate dormant cracks, but does slow actively growing cracks (due to introduction of compressive zone ahead of crack). Reference Associated SCC Guideline Been et al. (2006) N-III-3, N-III-5 Been et al. (2006) N-III-3, N-III-5 Been et al. (2006) Been et al. (2006) N-0-10, N-IV-4 Beavers (2004)
research reportNot linked to a paper · refsec
N-III-3 Beavers (2004) N-III-8, N-III-9 Beavers (2004) N-III-2, N-III-9 Beavers (2004)
research reportNot linked to a paper · refsec
Beavers (2004) continued …. - B-45 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. R&D Guideline Reference Associated SCC Guideline Beavers (2004) N-III-8, N-III-9 Beavers (2004) N-III-9, N-III-10 A critical crack-tip strain rate exists below which cracks go dormant. The value of the critical crack-tip strain rate is uncertain because of variability in models to
government reportNot linked to a paper · refsec
SSRT ductility. There is no single soil extract parameter that correlates with SCC susceptibility. Conclusion is that there is unlikely to be a single parameter that can be used to rank SCC sites. More-negative ECORR (native potential) and redox potential is an indicator of higher susceptibility (as measured by SSRT and H-perm). Suggestion is that native potentials could be used as a measure of susceptibility. Consistent with observation of more-negative redox potentials at field SCC sites. Reference Associated SCC Guideline Beavers (2004) Jack et al. (1999) Zheng et al. (1995) N-II-1 Watson et al. (1996) N-0-9 PsailaDombrowski et al. (1997) N-IV-11 King et al. (2004a) King et al. (2004a) N-I-2 King et al. (2004a) N-I-1 continued …. - B-47 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N176 N177 N178 N179 N180 N181 N182 N183 R&D Guideline
datasetNot linked to a paper · refsec
CP. Based on experimental observation using simulated disbondment and application of CP with and without CO2 purge. Gradation of corrosion damage along disbondment due to potential gradient. Less corrosion near mouth, pitting at intermediate locations, and general corrosion furthest from mouth. Penetration of CP will depend on various factors, including: disbondment height, current density, conductivity of solution, physical/spatial restrictions. Under cyclic loading, pits in disbonded region nucleate cracks. Cracks initiate some distance away from disbondment mouth at location where pits nucleate. Initial surface condition of steel plate unknown. Cyclic loading can induce a burst of room-temperature creep of pipeline steels. Creep burst could have significance for crack initiation and growth for both high-pH and NNpH SCC. Aggressive soils exhibit a narrow range of pH as a function of CO2 partial pressure. May indicate that highly buffered solutions are more aggressive. However, in this study aggressiveness was determined by TTF of SSRT, so question of what is being measured. Reference Associated SCC Guideline Van Boven et al. (2007b)
research reportNot linked to a paper · refsec
SCC colonies associated with mean maximum sub-surface (0-2 mm) residual stress of 220 MPa. Maximum residual stress corresponds to plateau value observed at depths between ~1-2 mm. No SCC colonies associated with mean maximum sub-surface (0-2 mm) residual stress of 100 MPa. Maximum residual stress corresponds to plateau value observed at depths between ~1-2 mm. Reference Associated SCC Guideline Beavers et al. (2001) Beavers et al. (2001) Beavers et al. (2001) N-I-5 Beavers et al. (2001) Beavers et al. (2001) Beavers et al. (2000) N-I-11, N-III-12 Beavers et al. (2000) N-III-12 Beavers et al. (2000) N-I-11, N-III-12 Beavers et al. (2000) N-I-11 continued …. - B-57 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N254 N255 N256 N257 N258 N259 N260 N261 N262 N263 R&D Guideline Increased microhardness levels show weak correlation with SCC colonies. Evidence for some correlation between increasing microhardness and SCC colonies, but correlation is weak. Rougher surfaces associated with SCC colonies. Increased probability of finding
datasetNot linked to a paper · refsec
Parkins (1992) Associated SCC Guideline N-0-4 N-0-2 Parkins (1992)
research reportNot linked to a paper · refsec
N-I-8 Parkins (1999) N-I-8 continued …. - B-63 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N311 N312 N313 N314 N315 N316 N317 N318 N319 N320 N321 N322 R&D Guideline Uncertain whether new multilayer coatings will support NNpH SCC. Such coatings may exhibit apparently beneficial effects of FBE and/or the surface prep required to apply FBE or the detrimental effects of tape coating Do Cl- and SO42- play an active role in NNpH SCC? Cracking can be obtained in pure water purged with CO2, yet all trapped waters contain Cl- and sulphate. Crack initiation is not random, but is directed. Cracks often initiate just ahead of existing crack tips, or around periphery of un-corroded area with pit in centre, or adjacent to tape coating. Dormant cracks can be reactivated if they coalesce with growing crack. Static load near yield stress is insufficient to initiate cracks. Pipelines operating
datasetNot linked to a paper · refsec
SCC. Preliminary study, careful about over-interpreting. Bending stress more important for crack on shoulder on an unconstrained dent than the hoop stress. Implies cracks associated with dents will grow in non-axial orientations Hydrotest procedure will not necessarily slow the subsequent growth of cracks in a dent. Based on CTOD observations of effect of simulation hydrotest on growth in air of crack on shoulder of unconstrained dent. Reference Associated SCC Guideline Parkins (1999)
research reportNot linked to a paper · refsec
N-III-9 Parkins (1999) N-0-3, N-II-2 Parkins (1999)
research reportNot linked to a paper · refsec
N-I-19 Parkins (1999) N-0-9 Davis and Parkins (1992) Brongers et al. (2009) N-I-12 Brongers et al. (2009) continued …. - B-64 -
research reportNot linked to a paper · refsec
SCC, than FBE For shielding coatings, bare area adjacent to disbondment prevents any protection under disbondment. Thus, for PE ctg, a bare area will be preferentially polarised with no CP reaching disbondment. However, bare area has less effect of distribution of current for CTE which is generally permeable. Inadequate grit blasting can lead to no improvement in SCC resistance. Appear to require a white surface finish, rather than near-white, to ensure sufficient grit blasting to prevent SCC. Older FBE lines may have been inadequately blasted. Cracks in dense crack patches tend to become dormant because of shielding by neighbouring cracks. Dense patches defined as those with a crack spacing of <20% of the wall thickness) Cracks in sparse crack patches can continue to grow unhindered by shielding. A crack patch is not the same as a crack colony, the latter being more defined by the shape and size of the disbondment. Complex 3-D interaction of stress within a crack patch with the crack-tip stress increasing, decreasing, or remaining constant with increasing depth under various circumstances. High-pH and NNpH SCC cracks show similar characteristics in terms of crack size, spacing, and shape Reference Associated SCC Guideline Beavers (1992)
research reportNot linked to a paper · refsec
Beavers (1992) N-I-8 Leis and Colwell (1997) N-III-8 Leis and Colwell (1997) N-III-14, N-IV-10 Leis and Colwell (1997) Leis and Colwell (1997) continued …. - B-65 -
government reportNot linked to a paper · refsec
SCC for cracks away from the failure but show no clear trend with depth for cracks that lead to failure. Hydrogen plays a significant role in NNpH SCC, but the mechanism has not been identified. In a correlative site-selection model for a single pipeline, three parameters were found to be key predictors of NNpH SCC: pipe manufacturer, coating type, and soil type.  >4 times more likely to find SCC in glaciofluvial soil than in lacustrine soil  >3 times more likely to find SCC under asphalt coating compared with other coatings (CTE, epoxy urethane, FBE, tape, wax)  >18 times more likely for pipe from manufacturer G to exhibit SCC than pipe from manufacturers A, B, or C Susceptibility to NNpH SCC increases with decreasing O2 concentration. Dissolution of millscale can lead to axially aligned corrosion pits or trenches which act as ideal crack initiation sites Millscale is electrochemically active and participates in the crack initiation and growth process. Although there is no evidence in support or contrary, millscale may exhibit varying electrochemical activity resulting in varying susceptibility. Van Boven et al. (2002) Castaneda et al. (2008) Associated SCC Guideline N-0-8 Castaneda et al. (2008) Castaneda et al. (2008)
research reportNot linked to a paper · refsec
ASME. 2004. Integrity Management of Stress Corrosion Cracking in Gas Pipeline High Consequence Areas. ASME Standards Technology Publication STP-PT-011, American Society for Mechanical Engineers (New York, NY).
research reportNot linked to a paper · refsec
ASTM. 2005. ASTM Standard E1049-85(2005), Standard Practices for Cycle Counting in Fatigue. ASTM International, West Conshohocken, PA, 2006, DOI: 10.1520/E104985R05.
journal articleNot linked to a paper · refsec
Baker. 2005. Stress Corrosion Cracking Study. Prepared by Michael Baker Jr., Inc. for the U.S. Department of Transportation, Office of Pipeline Safety. TTO Number 8, Integrity Management Program Delivery Order DTRS56-02-D-70036.
research reportNot linked to a paper · refsec
Beavers, J.A. and W.V. Harper. 2004. Stress corrosion cracking prediction model. Proc.
government reportNot linked to a paper · refsec
Beavers, J.A. and R.G. Worthingham. 2002. The influence of soil chemistry on SCC of underground pipelines. Proc. 4th International Pipeline Conference (ASME, New York,
government reportNot linked to a paper · refsec
NY), paper IPC2002-27146. Beavers, J.A., J.T. Johnson, and R.L. Sutherby. 2000. Materials factors influencing the initiation of near-neutral pH SCC on underground pipelines. Proc. International Pipeline
research reportNot linked to a paper · refsec
CEPA. 1998. CEPA Stress Corrosion Cracking Database: First Trending Report. Canadian Energy Pipeline Association (Calgary, AB).
datasetNot linked to a paper · refsec
CEPA. 2000. CEPA Stress Corrosion Cracking Database: Second Trending Report. Canadian Energy Pipeline Association (Calgary, AB).
datasetNot linked to a paper · refsec
King, F., G. Van Boven, T.R. Jack, R. Sutherby, and L. Fenyvesi. 2003. Predicting the growth of low- and high-pH SCC on gas transmission pipelines based on operating conditions. In Proc. CORROSION/2003 Research Topical Symposium: Modeling and Prediction of Lifetimes for Corrodible Structures, J.R. Scully and D.W. Shoesmith (eds.), NACE International (Houston, TX), pp. 127-155. - C-40 King, F., K. Ikeda-Cameron, T. Jack, and J. Been. 2004. Long-term environmental monitoring of near-neutral and high-pH SCC sites and the basis of an improved SCC site selection model. Gas Research Institute Report, GRI-04/0098.
research reportNot linked to a paper · refsec
Leeson, R. and D.K. Spitzmacher. 2006. SCC inspection & mitigation program on Suncor
research reportNot linked to a paper · refsec
Penner, L., G. Mollard, M. Holm, and R. Sutherby. 2003. Geological, geotechnical and hydrogeological setting of a gas pipeline failure near Brandon, Manitoba. In Proc. 56th Annual Canadian Geotech. Conf., Canadian Geotechnical Society (Ottawa, ON)
research reportNot linked to a paper · refsec
Inquiry, NEB Report MH-2-95. National Energy Board (Calgary, AB). Van Boven, G., R. Sutherby, and F. King. 2002. Characterizing pressure fluctuations on buried pipelines in terms relevant to stress corrosion cracking. Proc. 4th International Pipeline Conference (ASME, New York, NY), paper IPC2002-27149. Van Boven, G., T.R. Jack, and F. King. 2004. Environmental factors: effect on SCC growth. Gas Research Institute Report, GRI-04/0161.