{"document":{"doc_id":142866,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"PHMSA R and D Guidelines for the Identification of SCC Sites and the Estimation of Re-inspection Intervals for SCCDA","date":"2023-09-20","url":"https://www.regulations.gov/document/PHMSA-2011-0023-0757","source_native_id":"PHMSA-2011-0023-0757","status":"fetched","abstract":null,"action":null},"dockets":["PHMSA-2011-0023"],"rins":["RIN 2137-AE72","RIN 2137-AF39","RIN 2137-AF38"],"related":[{"doc_id":13699,"source":"fr_rule","org":"DEPARTMENT OF TRANSPORTATION; Pipeline and Hazardous Materials Safety Administration","doc_type":"Proposed Rule","title":"Pipeline Safety: Safety of Gas Transmission Pipelines","date":"2011-08-25"},{"doc_id":147048,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"The Interstate Natural Gas Association of America and the American Gas Association - Request","date":"2011-09-19"},{"doc_id":147046,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"Texas Pipeline Association - Request for Extension","date":"2011-09-28"},{"doc_id":147047,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"Interstate Natural Gas Association of America's & American Gas Association's","date":"2011-09-28"},{"doc_id":13463,"source":"fr_rule","org":"DEPARTMENT OF TRANSPORTATION; Pipeline and Hazardous Materials Safety Administration","doc_type":"Proposed Rule (administrative)","title":"Pipeline Safety: Safety of Gas Transmission Pipelines","date":"2011-11-16"},{"doc_id":159842,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"Interstate Natural Gas Association of America - Letter","date":"2011-12-27"},{"doc_id":159841,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"Stephen and Tina Henning - Comments","date":"2012-01-31"},{"doc_id":147045,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"INGAA ANPRM Safety of Gas Transmission Pipelines Webinar","date":"2012-02-10"},{"doc_id":147044,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"U.S. DOT/PHMSA - Meeting with PHMSA and INGAA to discuss comments on Pipeline Safety: Safety of Gas Transmission Pipelines","date":"2012-10-10"},{"doc_id":147043,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"American Petroleum Institute - Comment","date":"2012-11-02"},{"doc_id":146054,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"Supporting Document forGas Transmission for NPRM","date":"2016-04-07"},{"doc_id":9906,"source":"fr_rule","org":"DEPARTMENT OF TRANSPORTATION; Pipeline and Hazardous Materials Safety Administration","doc_type":"Proposed Rule","title":"Pipeline Safety: Safety of Gas Transmission and Gathering Pipelines","date":"2016-04-08"},{"doc_id":160701,"source":"docket_item","org":"PHMSA","doc_type":"other","title":"National Association of Pipeline Safety Representatives Request  for Extension- NAPSR 4-8-2016 Sub","date":"2016-04-11"},{"doc_id":159177,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"CONSOL Energy Inc. Letter  -  Extension Request U.S DOT PipelineSafety 04192016","date":"2016-04-19"},{"doc_id":160696,"source":"docket_item","org":"PHMSA","doc_type":"other","title":"Southwest Gas Corporation - Request for Extension of Comment Period","date":"2016-05-03"},{"doc_id":160697,"source":"docket_item","org":"PHMSA","doc_type":"other","title":"Pennsylvania Public Utility Commission - Request for Extension of Comment Period","date":"2016-05-03"},{"doc_id":159174,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"AGA, INGAA, API, IPAA, GPA, and APGA- Request for Extension of Comment Period","date":"2016-05-10"},{"doc_id":159175,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"New York State of Opportunity Department of Public Service - Extenson of Time Request","date":"2016-05-10"},{"doc_id":159176,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"Marcellus Shale Coalitition -   Extension Request","date":"2016-05-10"},{"doc_id":9842,"source":"fr_rule","org":"DEPARTMENT OF TRANSPORTATION; Pipeline and Hazardous Materials Safety Administration","doc_type":"Proposed Rule (administrative)","title":"Pipeline Safety: Safety of Gas Transmission and Gathering Pipelines","date":"2016-05-13"},{"doc_id":146048,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"U.S. DOT/PHMSA - Report to Congress - Evaluation of Expanding Pipeline Integrity Management Beyond High-Consequence Areas and Whether Such Expansion Would Mitigate the Need for Gas Pipeline Class Location Requirements - Pipeline Safety, Regulatory Certainty, And Job Creation Act 2011, Section 5","date":"2016-06-09"},{"doc_id":160684,"source":"docket_item","org":"PHMSA","doc_type":"other","title":"NAPSR  - 2016 GasTrans NPRM Extension Request Ltr NAPSR 6-21-2016 Submitted","date":"2016-06-27"},{"doc_id":146046,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"Safety of Gas Trans Appendix","date":"2016-07-12"},{"doc_id":146045,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"U.S DOT/PHMSA - Comments of Peoples Natural Gas Company, LLC","date":"2016-07-26"},{"doc_id":159147,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"U.S. DOT/PHMSA - Notes from Meeting with Pennsylvania Grade Crude Oil Coalition","date":"2017-03-24"},{"doc_id":146035,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"The  Interstate Natural Gas Association of America (INGAA) - Report - Analysis of Natural Gas Transmission Pipeline Releases and Mitigation Options for Pipeline MAOP Reconfirmation","date":"2017-04-21"},{"doc_id":146029,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"Gas Pipeline Advisory Committee Meeting","date":"2017-12-01"},{"doc_id":146030,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"Gas Pipeline Advisory Committee Meeting Pre-briefing on December 5","date":"2017-12-01"},{"doc_id":146028,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"U.S. DOT/NHTSA - Final Report  - 2017 Mitsubishi Outlander","date":"2018-03-08"},{"doc_id":146027,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"U.S. DOT/PHMSA - Gas Pipeline Advisory Committee Meeting","date":"2018-03-19"},{"doc_id":159135,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"GPAC-Slide Presentation Gas Rule - March 26 to 28 Mtg #5-FINAL","date":"2018-04-16"},{"doc_id":145981,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"GPAC- Gas Gathering Pre-brief presentation","date":"2018-12-26"},{"doc_id":159130,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"Pipeline Safety: Safety of Gas Transmission Pipelines","date":"2018-12-26"},{"doc_id":159123,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"U.S. DOT/PHMSA - Letters - November 15, 2018, October 10, 2018, Meeting of PHMSA Personnel with Representatives of the Gathering Line Industry","date":"2019-02-15"},{"doc_id":145969,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"Gas Pipeline Advisory Committee Meeting Pre-brief June 19, 2019","date":"2019-07-16"},{"doc_id":145970,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"GPAC Approved Gas Gathering Lines Vote Slides for June 25-26, 2019 Meeting","date":"2019-07-16"},{"doc_id":145971,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"Gas Pipeline Advisory Committee Meeting Slides for June 25-26, 2019","date":"2019-07-16"},{"doc_id":7498,"source":"fr_rule","org":"DEPARTMENT OF TRANSPORTATION; Pipeline and Hazardous Materials Safety Administration","doc_type":"Rule","title":"Pipeline Safety: Safety of Gas Transmission Pipelines: MAOP Reconfirmation, Expansion of Assessment Requirements, and Other Related Amendments","date":"2019-10-01"},{"doc_id":7191,"source":"ria","org":"PHMSA","doc_type":"regulatory_impact_analysis","title":"Gas Transmission Regulatory Impact Analysis","date":"2019-10-02"},{"doc_id":129370,"source":"docket_item","org":"PHMSA","doc_type":"review_record","title":"Substantive Differences Between the Final Rule Submitted to OIRA on May 21, 2019, and Published in the Federal Register on October 1, 2019, pursuant to EO 12866 Sec. 6(a)(3)(E)","date":"2019-10-02"},{"doc_id":145514,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"Final Regulatory Flexibility Act (RFA) Small Business","date":"2019-10-02"},{"doc_id":145515,"source":"docket_item","org":"PHMSA","doc_type":"other","title":"Gas Transmission Final Environmental Assessment","date":"2019-10-02"},{"doc_id":145507,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"GT Final Rule - GT GG Annual Report and Instructions","date":"2019-10-24"},{"doc_id":145508,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"GT Final Rule - GT GG Incident Report and Instructions","date":"2019-10-24"},{"doc_id":158708,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"Summary of Meeting with GPA Midstream on March 29, 2019","date":"2019-11-19"},{"doc_id":145137,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"API Petition Grant Response Letter","date":"2020-03-10"},{"doc_id":145138,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"APGA Petition Grant Response Lette","date":"2020-03-10"},{"doc_id":145139,"source":"docket_item","org":"PHMSA","doc_type":"report","title":"APGA Petition Grant Response Letter","date":"2020-03-10"},{"doc_id":158492,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"AGA Petition Grant Response Letter","date":"2020-03-10"},{"doc_id":6917,"source":"fr_rule","org":"DEPARTMENT OF TRANSPORTATION; Pipeline and Hazardous Materials Safety Administration","doc_type":"Rule","title":"Pipeline Safety: Safety of Gas Transmission Pipelines: MAOP Reconfirmation, Expansion of Assessment Requirements, and Other Related Amendments: Response to a Joint Petition for Reconsideration","date":"2020-07-06"},{"doc_id":158355,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"Meeting with PST  dated 2-11-21","date":"2021-03-13"},{"doc_id":158281,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"EO12866 Meeting - Gas Gathering - API - 10.4.21","date":"2021-10-13"},{"doc_id":158283,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"EO12866 Meeting Summary - Gas Gathering - GPA 10.5.21","date":"2021-10-13"},{"doc_id":158266,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"National Registry Notification Instructions - PHMSA F1000.2 (rev 1-2020) Clean 2021-07-29","date":"2021-11-12"},{"doc_id":158267,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"Gas Gathering Final Rule- Substantive Changes from EO12866 Review","date":"2021-11-12"},{"doc_id":158268,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"EA Safety of Gas Gathering Pipelines Final Rule","date":"2021-11-12"},{"doc_id":158269,"source":"docket_item","org":"PHMSA","doc_type":"correspondence","title":"AFPA Briefing to PHMSA 7-16-19","date":"2021-11-12"},{"doc_id":7188,"source":"ria","org":"PHMSA","doc_type":"regulatory_impact_analysis","title":"Final RIA/RFA: Safety of Gas Gathering Pipelines","date":"2021-11-14"},{"doc_id":155491,"source":"docket_item","org":"PHMSA","doc_type":"other","title":"Final Gas Gathering Forms - Redlines","date":"2021-11-14"},{"doc_id":155492,"source":"docket_item","org":"PHMSA","doc_type":"other","title":"Final Gas Gathering Forms and Instructions - Clean","date":"2021-11-14"}],"references":[{"citation_id":1560530,"raw_reference":"API. 2000. API Recommended Practice 579, Fitness for Service. American Petroleum Institute (Washignton, DC)","cited_authors":"API","cited_year":"2000","cited_title":"API Recommended Practice 579, Fitness for Service","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560531,"raw_reference":"ASME. 2004. Managing System Integrity of Gas Pipelines. ASME Code for Pressure Piping, B31. Supplement to ASME B31.8. American Society for Mechanical Wngineers (New","cited_authors":"ASME","cited_year":"2004","cited_title":"Managing System Integrity of Gas Pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560532,"raw_reference":"York, NY). Beavers, J.A. and C.L. Durr. 2000. Cathodic protection conditions conducive to SCC. Report prepared for the Corrosion Supervisory Committee, Pipeline Research Council","cited_authors":"York, NY). Beavers, J.A. and C.L. Durr","cited_year":"2000","cited_title":"Cathodic protection conditions conducive to SCC. Report prepared for the Corrosion Supervisory Committee, Pipeline Research Council","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560533,"raw_reference":"International, Catalo No. L51897. Beavers, J.A. and R.G. Worthingham. 2002. The influence of soil chemistry on SCC of underground pipelines. Proc. 4th International Pipeline Conference (ASME, New York,","cited_authors":"International, Catalo No. L51897. Beavers, J.A. and R.G. Worthingham","cited_year":"2002","cited_title":"The influence of soil chemistry on SCC of underground pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560534,"raw_reference":"NY), paper IPC2002-27146. Beavers, J.A., C.L. Durr, and B.S. Delanty. 1998. High-pH SCC: temperature and potential dependence for cracking in field environments. Proc. IPC 1998, ASME (New York, NY), Vol. 1, pp. 423-437.","cited_authors":"NY), paper IPC2002-27146. Beavers, J.A., C.L. Durr, and B.S. Delanty","cited_year":"1998","cited_title":"High-pH SCC: temperature and potential dependence for cracking in field environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560535,"raw_reference":"Beavers, J.A., J.T. Johnson, and R.L. Sutherby. 2000. Materials factors influencing the initiation of near-neutral pH SCC on underground pipelines. Proc. International Pipeline","cited_authors":"Beavers, J.A., J.T. Johnson, and R.L. Sutherby","cited_year":"2000","cited_title":"Materials factors influencing the initiation of near-neutral pH SCC on underground pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560536,"raw_reference":"Conf. 2000 (ASME International, New York, NY), vol. 2, pps. 979-988.","cited_authors":null,"cited_year":null,"cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560537,"raw_reference":"CEPA. 2007. Stress Corrosion Cracking. Recommended Practices, 2nd Edition. Canadian Energy Pipeline Association (Calgary, AB).","cited_authors":"CEPA","cited_year":"2007","cited_title":"Stress Corrosion Cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560538,"raw_reference":"King, F., T. Jack, M. Kolar, and R. Worthingham. 2004. A permeable coating model for predicting the environment at the pipe surface under CP-compatible coatings. Proc. 5th International Pipeline Conference (ASME, New York, NY), paper IPC04-0368.","cited_authors":"King, F., T. Jack, M. Kolar, and R. Worthingham","cited_year":"2004","cited_title":"A permeable coating model for predicting the environment at the pipe surface under CP-compatible coatings","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560539,"raw_reference":"NACE. 2008. Stress Corrosion Cracking (SCC) Direct Assessment Methodology. Standard","cited_authors":"NACE","cited_year":"2008","cited_title":"Stress Corrosion Cracking (SCC) Direct Assessment Methodology","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560540,"raw_reference":"Practice, SP0204-2008. NACE International (Houston, TX).","cited_authors":null,"cited_year":null,"cited_title":"Practice, SP0204-2008","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560541,"raw_reference":"NEB. 1996. Stress Corrosion Cracking on Canadian Oil and Gas Pipelines, Report of the","cited_authors":"NEB","cited_year":"1996","cited_title":"Stress Corrosion Cracking on Canadian Oil and Gas Pipelines, Report of the","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560542,"raw_reference":"Parkins, R.N. 1994. Overview of intergranular stress corrosion cracking research activities. Report to Line Pipe Research Supervisory Committee of the American Gas Association,","cited_authors":"Parkins, R.N","cited_year":"1994","cited_title":"Overview of intergranular stress corrosion cracking research activities","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560543,"raw_reference":"Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 323-333 Relevant phase(s) in SCC Guidelines: Susceptibility Sub-phase/keywords: Soil type, large-diameter, gas transmission, tape coating, SCC failures, groundwater, pH, redox potential, near-neutral pH SCC, correlation, land use, Russian Results support R&D Guideline no.: Comments: This paper describes Russian experience with developing a “soils model” based on field observations at","cited_authors":"Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam","cited_year":"2008","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560544,"raw_reference":"Ahmed, T.M., S.B. Lambert, R. Sutherby, and A. Plumtree. 1997. Cyclic crack growth rates of X-60 pipeline steel in a neutral dilute solution. Corrosion 53(7).","cited_authors":"Ahmed, T.M., S.B. Lambert, R. Sutherby, and A. Plumtree","cited_year":"1997","cited_title":"Cyclic crack growth rates of X-60 pipeline steel in a neutral dilute solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560545,"raw_reference":"Armstrong, R.D. and A.C. Coates. 1976. A correlation between electrochemical parameters and stress corrosion cracking. Corrosion Science 16, 423-433.","cited_authors":"Armstrong, R.D. and A.C. Coates","cited_year":"1976","cited_title":"A correlation between electrochemical parameters and stress corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"journal_article","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560546,"raw_reference":"Asahi, H., T. Kushida, M. Kimura, H. Fukai, and S. Okano. 1996. The investigation on stress corrosion cracking in a carbonate-bicarbonate solution and its mechanism from metallurgical aspects. Proc. 9th Linepipe Symposium, Pipeline Research Council","cited_authors":"Asahi, H., T. Kushida, M. Kimura, H. Fukai, and S. Okano","cited_year":"1996","cited_title":"The investigation on stress corrosion cracking in a carbonate-bicarbonate solution and its mechanism from metallurgical aspects","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560547,"raw_reference":"Asahi, H., T. Kushida, M. Kimura, H. Fukai, and S. Okano. 1999. Role of microstructures on stress corrosion cracking of pipeline steels in carbonate-bicarbonate solution. Corrosion 55, 644-652.","cited_authors":"Asahi, H., T. Kushida, M. Kimura, H. Fukai, and S. Okano","cited_year":"1999","cited_title":"Role of microstructures on stress corrosion cracking of pipeline steels in carbonate-bicarbonate solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560548,"raw_reference":"Asher, S.L. and P.M. Singh. 2009. Role of stress in transgranular stress corrosion cracking of transmission pipelines in near-neutral pH environments. Corrosion 65(2), 79-87.","cited_authors":"Asher, S.L. and P.M. Singh","cited_year":"2009","cited_title":"Role of stress in transgranular stress corrosion cracking of transmission pipelines in near-neutral pH environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560549,"raw_reference":"Atrens, A., Z.F. Wang, N. Kinaev, D.R. Cousens, and J.Q. Wang. 1996. Applicability of ESEM in SCC studies. Proc. 13th Int. Corrosion Congress, Melbourne, Australia, paper no. 233.","cited_authors":"Atrens, A., Z.F. Wang, N. Kinaev, D.R. Cousens, and J.Q. Wang","cited_year":"1996","cited_title":"Applicability of ESEM in SCC studies","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560550,"raw_reference":"Beavers, J.A. 1992. Assessment of the effects of surface preparation and coatings on the susceptibility of line pipe to stress-corrosion cracking. Report to Corrosion Supervisory","cited_authors":"Beavers, J.A","cited_year":"1992","cited_title":"Assessment of the effects of surface preparation and coatings on the susceptibility of line pipe to stress-corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560551,"raw_reference":"Committee, PR186-917, Final Report. Beavers, J.A. 2004. Near-neutral pH SCC: dormancy and re-initiation of stress corrosion cracks. Gas Research Institute Report GRI-7045.","cited_authors":"Committee, PR186-917, Final Report. Beavers, J.A","cited_year":"2004","cited_title":"Near-neutral pH SCC: dormancy and re-initiation of stress corrosion cracks","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560552,"raw_reference":"Beavers, J.A. and E.L. Hagerdorn. 1996. Near-neutral pH SCC: mechanical effects on crack propagation. Proc. 9th Linepipe Symposium, Pipeline Research Council International, Catalog No. L51746, paper 24.","cited_authors":"Beavers, J.A. and E.L. Hagerdorn","cited_year":"1996","cited_title":"Near-neutral pH SCC: mechanical effects on crack propagation","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560553,"raw_reference":"Beavers, J.A. and C.E. Jaske. 1998. Near-neutral pH SCC in pipelines: effects of pressure fluctuations on crack propagation. Proc. CORROSION/98, NACE International (Houston, TX), paper no. 257.","cited_authors":"Beavers, J.A. and C.E. Jaske","cited_year":"1998","cited_title":"Near-neutral pH SCC in pipelines: effects of pressure fluctuations on crack propagation","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560554,"raw_reference":"Beavers, J.A. and C.L. Durr. 2000. Cathodic protection conditions conducive to SCC. Report prepared for the Corrosion Supervisory Committee, Pipeline Research Council","cited_authors":"Beavers, J.A. and C.L. Durr","cited_year":"2000","cited_title":"Cathodic protection conditions conducive to SCC. Report prepared for the Corrosion Supervisory Committee, Pipeline Research Council","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560555,"raw_reference":"NY), paper IPC2002-27146. Beavers, J.A. and C.E. Jaske. 2004. Effects of pressure fluctuations on SCC propagation. Pipeline Research Council International Report, Catalog no. L51872e. - A-228 Beavers, J.A. and W.V. Harper. 2004. Stress corrosion cracking prediction model. Proc.","cited_authors":"NY), paper IPC2002-27146. Beavers, J.A. and C.E. Jaske","cited_year":"2004","cited_title":"Effects of pressure fluctuations on SCC propagation","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560556,"raw_reference":"CORROSION/2004, NACE International (Houston, TX), paper no. 04189.","cited_authors":null,"cited_year":null,"cited_title":"CORROSION/2004, NACE International (Houston, TX), paper no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560557,"raw_reference":"Beavers, J.A., R.N. Parkins, G.H. Koch, and W.E. Berry. 1985. Test method for defining susceptibility of line pipe steels to stress-corrosion cracking. Report to Line Pipe Research Supervisory Committee NG-18, Report No. 146.","cited_authors":"Beavers, J.A., R.N. Parkins, G.H. Koch, and W.E. Berry","cited_year":"1985","cited_title":"Test method for defining susceptibility of line pipe steels to stress-corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560558,"raw_reference":"Beavers, J.A., W.E. Berry, and R.N. Parkins. 1986. Standard test procedure for stress corrosion cracking threshold stress determination. Corrosion 42, 9-17.","cited_authors":"Beavers, J.A., W.E. Berry, and R.N. Parkins","cited_year":"1986","cited_title":"Standard test procedure for stress corrosion cracking threshold stress determination","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560559,"raw_reference":"Beavers, J.A., C.L. Durr, and S.S. Shademan. 1998. Mechanistic studies on near-neutral-pH","cited_authors":"Beavers, J.A., C.L. Durr, and S.S. Shademan","cited_year":"1998","cited_title":"Mechanistic studies on near-neutral-pH","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560560,"raw_reference":"Beavers, J.A., C.L. Durr, and B.S. Delanty. 1998. High-pH SCC: temperature and potential dependence for cracking in field environments. Proc. IPC 1998, ASME (New York, NY), Vol. 1, pp. 423-437.","cited_authors":"Beavers, J.A., C.L. Durr, and B.S. Delanty","cited_year":"1998","cited_title":"High-pH SCC: temperature and potential dependence for cracking in field environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560561,"raw_reference":"Beavers, J.A., C.L. Durr, B.S. Delanty, D.M. Owen, and R.L. Sutherby. 2001. Near-neutral pH","cited_authors":"Beavers, J.A., C.L. Durr, B.S. Delanty, D.M. Owen, and R.L. Sutherby","cited_year":"2001","cited_title":"Near-neutral pH","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560562,"raw_reference":"SCC: crack propagation in susceptible soil environments. Proc. CORROSION/2001,","cited_authors":null,"cited_year":null,"cited_title":"SCC: crack propagation in susceptible soil environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560563,"raw_reference":"Been, J., F. King, L. Yang, W. Chen, R. Sutherby, and R. Worthingham. 2003. Environmental effects on near-neutral pH SCC. Proc. Northern Area Western Conference, NACE International (Houston, TX), February 3-6, 2003, Calgary, AB, Canada.","cited_authors":"Been, J., F. King, L. Yang, W. Chen, R. Sutherby, and R. Worthingham","cited_year":"2003","cited_title":"Environmental effects on near-neutral pH SCC. Proc","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560564,"raw_reference":"Been, J., H. Lu, R. Eadie, G. Shen, and RT. Sutherby. 2004. The role of stress intensifiers in near-neutral pH corrosion fatigue of line pipe. Proc. CORROSION/2004, NACE International (Houston, TX), paper no. 04552.","cited_authors":"Been, J., H. Lu, R. Eadie, G. Shen, and RT. Sutherby","cited_year":"2004","cited_title":"The role of stress intensifiers in near-neutral pH corrosion fatigue of line pipe","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560565,"raw_reference":"Been, J., F. King, F. Song, and N. Sridhar. 2004. Coating deterioration as a precursor to SCC. Gas Research Institute Report, GRI-04/0099.","cited_authors":"Been, J., F. King, F. Song, and N. Sridhar","cited_year":"2004","cited_title":"Coating deterioration as a precursor to SCC. Gas Research Institute Report, GRI-04/0099","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560566,"raw_reference":"Been, J., L. Yang, H. Lu, and F. King. 2004. Inhibitive effects of organics on near-neutral pH","cited_authors":"Been, J., L. Yang, H. Lu, and F. King","cited_year":"2004","cited_title":"Inhibitive effects of organics on near-neutral pH","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560567,"raw_reference":"Been, J., F. King, L. Fenyvesi, and R. Sutherby. 2004. A modeling approach to high pH environmentally assisted cracking. Proc. 5th International Pipeline Conference (ASME, New York, NY), paper IPC04-0361.","cited_authors":"Been, J., F. King, L. Fenyvesi, and R. Sutherby","cited_year":"2004","cited_title":"A modeling approach to high pH environmentally assisted cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560568,"raw_reference":"Been, J., F. King, L. Yang, F. Song, and N. Sridhar. 2005. The role of coatings in the generation of high- and near-neutral pH environments that promote environmentally assisted cracking. Proc. CORROSION/2005, NACE International (Houston, TX), paper no. 05167. - A-229 Been, J., B. Carroll, A. Dinovitzer, and R. Sutherby. 2006. Stress intensification and crack growth in the presence of dents on pipelines. Proc. IPC 2006, ASME (New York, NY), paper IPC2006-10415.","cited_authors":"Been, J., F. King, L. Yang, F. Song, and N. Sridhar","cited_year":"2005","cited_title":"The role of coatings in the generation of high- and near-neutral pH environments that promote environmentally assisted cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560569,"raw_reference":"Been, J., R.R. Fessler, S. Keane, and W. Kresic. 2006. History of pressure fluctuations related to severity of near-neutral pH SCC. Proc. IPC 2006 (ASME, New York, NY), paper IPC2006-10412.","cited_authors":"Been, J., R.R. Fessler, S. Keane, and W. Kresic","cited_year":"2006","cited_title":"History of pressure fluctuations related to severity of near-neutral pH SCC. Proc","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560570,"raw_reference":"Been, J., R. Eadie, and R. Sutherby. 2006. Prediction of environmentally assisted cracking on gas and liquid pipelines. Proc. 6th International Pipeline Conference (ASME, New York,","cited_authors":"Been, J., R. Eadie, and R. Sutherby","cited_year":"2006","cited_title":"Prediction of environmentally assisted cracking on gas and liquid pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560571,"raw_reference":"NY), paper IPC2006-10345. Been, J., F. King, and R. Sutherby. 2008a. Environmentally assisted cracking of pipeline steels in near-neutral pH environments. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H.","cited_authors":"NY), paper IPC2006-10345. Been, J., F. King, and R. Sutherby","cited_year":"2008a","cited_title":"Environmentally assisted cracking of pipeline steels in near-neutral pH environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560572,"raw_reference":"Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 221-230.","cited_authors":"Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam","cited_year":"2008","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560573,"raw_reference":"Been, J., H. Lu, F. King, T. Jack, and R. Sutherby. 2008b. The role of hydrogen in EAC of pipeline steels in near-neutral pH environments. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H. Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 255-266.","cited_authors":"Been, J., H. Lu, F. King, T. Jack, and R. Sutherby","cited_year":"2008b","cited_title":"The role of hydrogen in EAC of pipeline steels in near-neutral pH environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560574,"raw_reference":"Blengino, J.M., M. Keddam, J.P. Labbe, and L. Robbiola. 1995. Physico-chemical characterization of corrosion layers formed on iron in a sodium carbonate-bicarbonate containing environment. Corros. Sci. 37, 621-643.","cited_authors":"Blengino, J.M., M. Keddam, J.P. Labbe, and L. Robbiola","cited_year":"1995","cited_title":"Physico-chemical characterization of corrosion layers formed on iron in a sodium carbonate-bicarbonate containing environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560575,"raw_reference":"Brongers, M.P.H. and J.A. Beavers. 2005. SCC in areas of local deformation. Gas Research Institute report GRI-04/0127.","cited_authors":"Brongers, M.P.H. and J.A. Beavers","cited_year":"2005","cited_title":"SCC in areas of local deformation","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560576,"raw_reference":"Brongers, M.P.H., W. Kovacs, C.S. Scott, and J.A. Beavers. 2009. Stress corrosion cracking in areas of local deformation. Pipeline Research Council International report, Catalog no.","cited_authors":"Brongers, M.P.H., W. Kovacs, C.S. Scott, and J.A. Beavers","cited_year":"2009","cited_title":"Stress corrosion cracking in areas of local deformation","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560577,"raw_reference":"TBD. Brousseau, R. and S. Qian. 1994. Distribution of steady-state cathodic currents underneath a disbonded coating. Corrosion 50 (12), 907-911.","cited_authors":"TBD. Brousseau, R. and S. Qian","cited_year":"1994","cited_title":"Distribution of steady-state cathodic currents underneath a disbonded coating","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560578,"raw_reference":"Bueno, A.H.S., B.B. Castri, and J.A.C. Ponciano. 2008. Assessment of stress corrosion cracking and hydrogen embrittlement susceptibility of buried pipeline steels. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H. Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 313-322.","cited_authors":"Bueno, A.H.S., B.B. Castri, and J.A.C. Ponciano","cited_year":"2008","cited_title":"Assessment of stress corrosion cracking and hydrogen embrittlement susceptibility of buried pipeline steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560579,"raw_reference":"Bulger, J. and J. Luo. 2000. Effect of microstructure on near-neutral-pH SCC. Proc. IPC 2000 (ASME, New York, NY), Vol. 2, pp. 947-952.","cited_authors":"Bulger, J. and J. Luo","cited_year":"2000","cited_title":"Effect of microstructure on near-neutral-pH SCC. Proc","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560580,"raw_reference":"Casteneda, H., B.N. Leis, and S.E. Rose. 2008. Report on model modules to assist assessing and controlling SCC. Report prepared for US Department of Transportation PHMSA, Contract DTRS56-05-T-0003. - A-230 Černý, I. and V. Linhart. 2004. An evaluation of the resistance of pipeline steels to initiation and early growth of stress corrosion cracks. Eng. Fract. Mech. 71, 913-921.","cited_authors":"Casteneda, H., B.N. Leis, and S.E. Rose","cited_year":"2008","cited_title":"Report on model modules to assist assessing and controlling SCC. Report prepared for US Department of Transportation PHMSA, Contract DTRS56-05-T-0003","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560581,"raw_reference":"Chen, W. and R. Sutherby. 2004. Environmental effect of crack growth rate of pipeline steel in near-neutral pH soil environments. Proc. International Pipeline Conf. 2004 (ASME","cited_authors":"Chen, W. and R. Sutherby","cited_year":"2004","cited_title":"Environmental effect of crack growth rate of pipeline steel in near-neutral pH soil environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560582,"raw_reference":"Chen, W. and R. Sutherby. 2006. Laboratory simulation of hydrostatic test in near-neutral pH soil environments. Proc. IPC 2006, ASME (New York, NY), paper IPC2006-10477.","cited_authors":"Chen, W. and R. Sutherby","cited_year":"2006","cited_title":"Laboratory simulation of hydrostatic test in near-neutral pH soil environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560583,"raw_reference":"Chen, W. and R.L. Sutherby. 2007. Crack growth behavior of pipeline steel in near-neutral pH soil environments. Met. Mater. Trans. A, 38A, 1260-1268.","cited_authors":"Chen, W. and R.L. Sutherby","cited_year":"2007","cited_title":"Crack growth behavior of pipeline steel in near-neutral pH soil environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560584,"raw_reference":"Chen, W., T.R. Jack, F. King, and M.J. Wilmott. 2000. Hydrogen permeation behavior of X-70 pipeline steel in a near-neutral pH soil environment. Proc. International Pipeline Conf. 2000 (ASME International, New York, NY), pp. 953-960.","cited_authors":"Chen, W., T.R. Jack, F. King, and M.J. Wilmott","cited_year":"2000","cited_title":"Hydrogen permeation behavior of X-70 pipeline steel in a near-neutral pH soil environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560585,"raw_reference":"Chen, W., F. King, and E. Vokes. 2002. Characteristics of near-neutral-pH stress corrosion cracks in an X-65 pipeline. Corrosion 58(3), 267-275.","cited_authors":"Chen, W., F. King, and E. Vokes","cited_year":"2002","cited_title":"Characteristics of near-neutral-pH stress corrosion cracks in an X-65 pipeline","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560586,"raw_reference":"Chen, W., F. King, T.R. Jack, and M.J. Wilmott. 2002. Environmental aspects of near-neutral pH stress corrosion cracking of pipeline steel. Met. Mat. Trans. A 33A, 1429-1436.","cited_authors":"Chen, W., F. King, T.R. Jack, and M.J. Wilmott","cited_year":"2002","cited_title":"Environmental aspects of near-neutral pH stress corrosion cracking of pipeline steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560587,"raw_reference":"Chen, W., S.-H. Wang, R. Chu, F. King, T.R. Jack, and R.R. Fessler. 2003. Effect of precyclic loading on stress-corrosion-cracking initiation in an X-65 pipeline steel exposed to nearneutral pH soil environment. Metall. Mater. Trans. A 34A, 2601-2608.","cited_authors":"Chen, W., S.-H. Wang, R. Chu, F. King, T.R. Jack, and R.R. Fessler","cited_year":"2003","cited_title":"Effect of precyclic loading on stress-corrosion-cracking initiation in an X-65 pipeline steel exposed to nearneutral pH soil environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560588,"raw_reference":"Chen, W., G, Van Boven, and R. Rogge. 2007b. The role of residual stress in neutral pH stress corrosion cracking of pipeline steels. Part II: crack dormancy. Acta Mater. 55, 43-53.","cited_authors":"Chen, W., G, Van Boven, and R. Rogge","cited_year":"2007b","cited_title":"The role of residual stress in neutral pH stress corrosion cracking of pipeline steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560589,"raw_reference":"Chen, W., R.L. Eadie, and R.L. Sutherby. 2008. Environmental effects on near-neutral pH stress corrosion cracking in pipelines. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H. Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 211220.","cited_authors":"Chen, W., R.L. Eadie, and R.L. Sutherby","cited_year":"2008","cited_title":"Environmental effects on near-neutral pH stress corrosion cracking in pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560590,"raw_reference":"Chen, W., R. Kania, R. Worthingham, and S. Kariyawasam. 2008. Crack growth model of pipeline steels in near-neutral pH soil environments. Proc. International Pipeline Conf. 2008 (ASME International, New York, NY), paper IPC2008-64475.","cited_authors":"Chen, W., R. Kania, R. Worthingham, and S. Kariyawasam","cited_year":"2008","cited_title":"Crack growth model of pipeline steels in near-neutral pH soil environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560591,"raw_reference":"Chen, W., H. Zhu, and S-H. Wang. 2009. Low temperature creep behaviour of pipeline steels. Can. Met. Quart. 48, 271-284.","cited_authors":"Chen, W., H. Zhu, and S-H. Wang","cited_year":"2009","cited_title":"Low temperature creep behaviour of pipeline steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560592,"raw_reference":"Chen, W., R. Kania, R. Worthingham, and G. Van Boven. 2009. Transgranular crack growth in the pipeline steels exposed to near-neutral pH soil aqueous solutions: the role of hydrogen. Acta Materialia 57, 6200-6214.","cited_authors":"Chen, W., R. Kania, R. Worthingham, and G. Van Boven","cited_year":"2009","cited_title":"Transgranular crack growth in the pipeline steels exposed to near-neutral pH soil aqueous solutions: the role of hydrogen","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560593,"raw_reference":"Chen, W., R. Kania, B. Worthingham, and S. Kariyawasam. 2009. Role of hydrogen in crack growth in pipeline steels exposed to near neutral pH soil environment. Proc. Int. Conf. on Fracture (ICF 12), Ottawa, ON, July 12-17, 2009, paper T19.005. - A-231 Chen, X., X.G. Li, C.W. Du, and Y.F. Cheng. 2009. Effect of cathodic protection on corrosion of pipeline steel under disbonded coating. Corrosion Science 51, 2242-2245.","cited_authors":"Chen, W., R. Kania, B. Worthingham, and S. Kariyawasam","cited_year":"2009","cited_title":"Role of hydrogen in crack growth in pipeline steels exposed to near neutral pH soil environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"journal_article","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560594,"raw_reference":"Cheng, Y.F. 2007. Fundamentals of hydrogen evolution reaction and its implications on nearneutral pH stress corrosion cracking of pipelines. Electrochim. Acta 52, 2661-2667.","cited_authors":"Cheng, Y.F","cited_year":"2007","cited_title":"Fundamentals of hydrogen evolution reaction and its implications on nearneutral pH stress corrosion cracking of pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560595,"raw_reference":"Cheng, Y.F. and L. Niu. 2007. Application of electrochemical techniques in investigation of the role of hydrogen in near-neutral pH stress corrosion cracking of pipelines. J. Mater. Sci. 42(10), 3425-3434.","cited_authors":"Cheng, Y.F. and L. Niu","cited_year":"2007","cited_title":"Application of electrochemical techniques in investigation of the role of hydrogen in near-neutral pH stress corrosion cracking of pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560596,"raw_reference":"Chu, R., W. Chen, S.-H. Wang, F. King, T.R. Jack, and R.R. Fessler. 2004. Microstructure dependence of stress corrosion cracking initiation in X-65 pipeline steel exposed to a near-neutral pH soil environment. Corrosion 60, 275-283.","cited_authors":"Chu, R., W. Chen, S.-H. Wang, F. King, T.R. Jack, and R.R. Fessler","cited_year":"2004","cited_title":"Microstructure dependence of stress corrosion cracking initiation in X-65 pipeline steel exposed to a near-neutral pH soil environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560597,"raw_reference":"Chudnovsky, A., B.-H. Choi, J. Fan, and B. Zhang. 2004. Application of the crack layer theory for understanding and modeling of stress corrosion cracking in high pressure pipeline steel. Gas Research Institute Report, GRI-04/0169.","cited_authors":"Chudnovsky, A., B.-H. Choi, J. Fan, and B. Zhang","cited_year":"2004","cited_title":"Application of the crack layer theory for understanding and modeling of stress corrosion cracking in high pressure pipeline steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560598,"raw_reference":"Colwell, J.A., B.N. Leis, and P.M. Singh. 2008. Crack initiation of line pipe steels in nearneutral pH environments. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H.","cited_authors":"Colwell, J.A., B.N. Leis, and P.M. Singh","cited_year":"2008","cited_title":"Crack initiation of line pipe steels in nearneutral pH environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560599,"raw_reference":"Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 233-242.","cited_authors":"Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam","cited_year":"2008","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560600,"raw_reference":"Danielson, M.J., R.H. Jones, and K. Krist. 2000. Effect of microstructure and microchemistry on the SCC behaviour of pipeline steels in a high pH environment. Proc.","cited_authors":"Danielson, M.J., R.H. Jones, and K. Krist","cited_year":"2000","cited_title":"Effect of microstructure and microchemistry on the SCC behaviour of pipeline steels in a high pH environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560601,"raw_reference":"CORROSION/2000, NACE International (Houston, TX), paper no. 00359.","cited_authors":null,"cited_year":null,"cited_title":"CORROSION/2000, NACE International (Houston, TX), paper no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560602,"raw_reference":"Danielson, M.J., R.H. Jones, and P. Dusek. 2001. Effect of microstructure and microchemistry on the SCC behavior of archival and modern pipeline steels in a high pH environment. Proc. CORROSION/2001, NACE International (Houston, TX), paper no. 01211.","cited_authors":"Danielson, M.J., R.H. Jones, and P. Dusek","cited_year":"2001","cited_title":"Effect of microstructure and microchemistry on the SCC behavior of archival and modern pipeline steels in a high pH environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560603,"raw_reference":"Davis, G.O. and R.N. Parkins. 1992. Microbial effects on stress-corrosion cracking of line-pipe steels in low-pH environments. Report to Line Pipe Research Supervisory Committee of the American Gas Association, NG-18 Report No. 202.","cited_authors":"Davis, G.O. and R.N. Parkins","cited_year":"1992","cited_title":"Microbial effects on stress-corrosion cracking of line-pipe steels in low-pH environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560604,"raw_reference":"Delafosse, D., B. Bayle, and C. Bosch. 2008. The roles of crack-tip plasticity, anodic dissolution and hydrogen of mild and C-Mn steels. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H. Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 267-278.","cited_authors":"Delafosse, D., B. Bayle, and C. Bosch","cited_year":"2008","cited_title":"The roles of crack-tip plasticity, anodic dissolution and hydrogen of mild and C-Mn steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560605,"raw_reference":"Eadie, R., L.W. Hunt, R. Sutherby, G. Roy, G. Shen, J. Luo, W. Chen. T.C. Hamré, F. King, and T. Jack. 2002. Long seam welds in gas and liquids pipelines and near-neutral pH stress corrosion cracking and corrosion fatigue. Proc. 4th International Pipeline Conference (ASME, New York, NY), paper IPC2002-27118.","cited_authors":"Eadie, R., L.W. Hunt, R. Sutherby, G. Roy, G. Shen, J. Luo, W. Chen. T.C. Hamré, F. King, and T. Jack","cited_year":"2002","cited_title":"Long seam welds in gas and liquids pipelines and near-neutral pH stress corrosion cracking and corrosion fatigue","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560606,"raw_reference":"Eadie, R.L., K.E. Szklarz, and R.L. Sutherby. 2003. Corrosion fatigue and near-neutral pH stress corrosion cracking of pipeline steel in very dilute carbonate/bicarbonate with and without the presence of hydrogen sulfide using the compliance technique. Proc.","cited_authors":"Eadie, R.L., K.E. Szklarz, and R.L. Sutherby","cited_year":"2003","cited_title":"Corrosion fatigue and near-neutral pH stress corrosion cracking of pipeline steel in very dilute carbonate/bicarbonate with and without the presence of hydrogen sulfide using the compliance technique","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560607,"raw_reference":"CORROSION/2003, NACE International (Houston, TX), paper no. 03527. - A-232 Eadie, R.L., K.E. Szklarz, and R.L. Sutherby. 2005. Corrosion fatigue and near-neutral pH stress corrosion cracking of pipeline steel and the effect of hydrogen sulfide. Corrosion 61(2), 167-173.","cited_authors":"CORROSION/2003, NACE International (Houston, TX), paper no. 03527. - A-232 Eadie, R.L., K.E. Szklarz, and R.L. Sutherby","cited_year":"2005","cited_title":"Corrosion fatigue and near-neutral pH stress corrosion cracking of pipeline steel and the effect of hydrogen sulfide","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560608,"raw_reference":"Eiber, R.J. and B.N. Leis. 1998. Protocol to prioritize sites for high-pH stress-corrosion cracking on gas pipelines. Report prepared for the Pipeline Corrosion Supervisory","cited_authors":"Eiber, R.J. and B.N. Leis","cited_year":"1998","cited_title":"Protocol to prioritize sites for high-pH stress-corrosion cracking on gas pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560609,"raw_reference":"Elboujdaini, M., Y.-Z. Wang, R.W. Revie, R.N. Parkins, and M.T. Shehata. 2000. Stress corrosion crack initiation processes: pitting and microcrack coalescence. Proc.","cited_authors":"Elboujdaini, M., Y.-Z. Wang, R.W. Revie, R.N. Parkins, and M.T. Shehata","cited_year":"2000","cited_title":"Stress corrosion crack initiation processes: pitting and microcrack coalescence","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560610,"raw_reference":"CORROSION/2000, NACE International (Houston, TX), paper no. 00379.","cited_authors":null,"cited_year":null,"cited_title":"CORROSION/2000, NACE International (Houston, TX), paper no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560611,"raw_reference":"Elboujdaini, M., Y.-Z. Wang, R.W. Revie, M. Shehata, G. de Silveira, and R.N. Parkins. 2005. Initiation of stress corrosion cracking in pipeline steel. Gas Research Institute Report,","cited_authors":"Elboujdaini, M., Y.-Z. Wang, R.W. Revie, M. Shehata, G. de Silveira, and R.N. Parkins","cited_year":"2005","cited_title":"Initiation of stress corrosion cracking in pipeline steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560612,"raw_reference":"GRI-05/0005. Fang, B., J. Wang, S. Xiao, E.-H. Han, Z. Zhu, and W. Ke. 2005. Stress corrosion cracking of X-70 pipeline steels by electropulsing treatment in near-neutral pH solution. J. Mater. Sci. 40(24), 6545-6552.","cited_authors":"GRI-05/0005. Fang, B., J. Wang, S. Xiao, E.-H. Han, Z. Zhu, and W. Ke","cited_year":"2005","cited_title":"Stress corrosion cracking of X-70 pipeline steels by electropulsing treatment in near-neutral pH solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560613,"raw_reference":"Fang, B., E.-H. Han, J. Wang, Z. Zhu, and W. Ke. 2006. Hydrogen in stress corrosion cracking of X-70 pipeline steels in near-neutral pH solutions. J. Mater. Sci. 41(6), 1797-1803.","cited_authors":"Fang, B., E.-H. Han, J. Wang, Z. Zhu, and W. Ke","cited_year":"2006","cited_title":"Hydrogen in stress corrosion cracking of X-70 pipeline steels in near-neutral pH solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560614,"raw_reference":"Fang, B., J.Q. Wang, E. Han, Z. Zhu, and W. Ke. 2008. Influence of strain rate on the stress corrosion cracking of X70 pipeline steel in dilute near-neutral pH solutions. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H. Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 303-311.","cited_authors":"Fang, B., J.Q. Wang, E. Han, Z. Zhu, and W. Ke","cited_year":"2008","cited_title":"Influence of strain rate on the stress corrosion cracking of X70 pipeline steel in dilute near-neutral pH solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560615,"raw_reference":"Fang, B., A. Eslami, R. Kania, R. Worthingham, J. Been, and W. Chen. 2008. Stress corrosion crack initiation in X-65 pipeline steel under disbonded coating with cathodic protection. Proc. IPC 2008, ASME (New York, NY), paper IPC2008-64476.","cited_authors":"Fang, B., A. Eslami, R. Kania, R. Worthingham, J. Been, and W. Chen","cited_year":"2008","cited_title":"Stress corrosion crack initiation in X-65 pipeline steel under disbonded coating with cathodic protection","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560616,"raw_reference":"Fang, B.Y., R.L. Eadie, W.X. Chen, and M. Elboujdaini. 2009. Pit to crack transition in X-52 pipeline steel in near neutral pH environment Part 1 – formation of blunt cracks from pits under cyclic loading. Corros. Eng. Sci. Technol. DOI 10.1179/147842208X386304.","cited_authors":"Fang, B.Y., R.L. Eadie, W.X. Chen, and M. Elboujdaini","cited_year":"2009","cited_title":"Pit to crack transition in X-52 pipeline steel in near neutral pH environment Part 1 – formation of blunt cracks from pits under cyclic loading","cited_venue":null,"cited_doi":"10.1179/147842208x386304","cited_url":null,"ref_kind":"journal_article","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560617,"raw_reference":"Fessler, R.R. 1976. Combination of conditions causes stress-corrosion cracking. Oil and Gas J. , February 16, 1976 edition, pp. 81-83.","cited_authors":"Fessler, R.R","cited_year":"1976","cited_title":"Combination of conditions causes stress-corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560618,"raw_reference":"Fessler, R.R., T.P. Groeneveld, and A.R. Elsea. 1977. Stress-corrosion and hydrogen-stress cracking in buried pipelines. In Proc. Stress Corrosion Cracking and Hydrogen Embrittlement of Iron Base Alloys, NACE-5, NACE International (Houston, TX), pp.135146.","cited_authors":"Fessler, R.R., T.P. Groeneveld, and A.R. Elsea","cited_year":"1977","cited_title":"Stress-corrosion and hydrogen-stress cracking in buried pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560619,"raw_reference":"Fletcher, A.A., L. Fletcher, and R.J. Morrison. 1983. The effect of pipe surface oxide upon crevice polarization and stress corrosion cracking under fusion bonded low density polyethylene coatings. Fifth Int. Conf. Internal and External Protection of Pipes,","cited_authors":"Fletcher, A.A., L. Fletcher, and R.J. Morrison","cited_year":"1983","cited_title":"The effect of pipe surface oxide upon crevice polarization and stress corrosion cracking under fusion bonded low density polyethylene coatings","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560620,"raw_reference":"Innsbruck, 25-27 October 1983, BHRA Fluid Engineering. - A-233 Francis, A. and C. Jandu. 2006. A new probabilistic model for high-pH stress-corrosion cracking. J. Pipeline Integrity 5, 5-24.","cited_authors":"Innsbruck, 25-27 October","cited_year":"1983","cited_title":"BHRA Fluid Engineering","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560621,"raw_reference":"Fu, A.Q. and Y.F. Cheng. 2009. Characterization of corrosion of X65 pipeline steel under disbonded coating by scanning Kelvin probe. Corrosion Science 51, 914-920.","cited_authors":"Fu, A.Q. and Y.F. Cheng","cited_year":"2009","cited_title":"Characterization of corrosion of X65 pipeline steel under disbonded coating by scanning Kelvin probe","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"journal_article","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560622,"raw_reference":"Fu, A.Q., X. Tang, and Y.F. Cheng. 2009. Characterization of corrosion of X70 pipeline steel in thin electrolyte layer under disbonded coating by scanning Kelvin probe. Corrosion Science 51, 186-190.","cited_authors":"Fu, A.Q., X. Tang, and Y.F. Cheng","cited_year":"2009","cited_title":"Characterization of corrosion of X70 pipeline steel in thin electrolyte layer under disbonded coating by scanning Kelvin probe","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"journal_article","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560623,"raw_reference":"Gabetta, G. 1997. Transgranular stress corrosion cracking of low-alloy steels in diluted solutions. Corrosion 53(7), 516-524.","cited_authors":"Gabetta, G","cited_year":"1997","cited_title":"Transgranular stress corrosion cracking of low-alloy steels in diluted solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560624,"raw_reference":"Gabetta, G., S. Di Liberto, and A. Bennardo. 2000. Laboratory tests reproduce transgranular stress corrosion cracking. Proc. CORROSION/2000 (NACE International, Houston, TX), paper no. 00372.","cited_authors":"Gabetta, G., S. Di Liberto, and A. Bennardo","cited_year":"2000","cited_title":"Laboratory tests reproduce transgranular stress corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560625,"raw_reference":"Gabetta, G., S. Di Liberto, A. Bennardo, and N. Mancini. 2001. Strain rate induced stress corrosion cracking in buried pipelines. Br. Corros. J. 36(1),24-28.","cited_authors":"Gabetta, G., S. Di Liberto, A. Bennardo, and N. Mancini","cited_year":"2001","cited_title":"Strain rate induced stress corrosion cracking in buried pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560626,"raw_reference":"Gangloff, R.P. 1985. Crack size effects on the chemical driving force for aqueous corrosion fatigue. Metall. Trans. A 16A, 953-969.","cited_authors":"Gangloff, R.P","cited_year":"1985","cited_title":"Crack size effects on the chemical driving force for aqueous corrosion fatigue","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560627,"raw_reference":"Gonzalez-Rodriguez, J.G., M. Casales, V.M. Salinas-Bravo, J.L. Albarran, and L. Martinez. 2002. Effect of microstructure on the stress corrosion cracking of X-80 pipeline steel in diluted sodium bicarbonate solutions. Corrosion 58(7), 584-590.","cited_authors":"Gonzalez-Rodriguez, J.G., M. Casales, V.M. Salinas-Bravo, J.L. Albarran, and L. Martinez","cited_year":"2002","cited_title":"Effect of microstructure on the stress corrosion cracking of X-80 pipeline steel in diluted sodium bicarbonate solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560628,"raw_reference":"Gu, B., J. Luo, and X. Mao. 1999. Hydrogen-facilitated anodic dissolution-type stress corrosion cracking of pipeline steels in near-neutral pH solution. Corrosion 55, 96-106.","cited_authors":"Gu, B., J. Luo, and X. Mao","cited_year":"1999","cited_title":"Hydrogen-facilitated anodic dissolution-type stress corrosion cracking of pipeline steels in near-neutral pH solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560629,"raw_reference":"Gu, B., W.Z. Yu, J.L. Luo, and X. Mao. 1999. Transgranular stress corrosion cracking of X-80 and X-52 pipeline steels in dilute aqueous solution with near-neutral pH. Corrosion 55(3), 312-318.","cited_authors":"Gu, B., W.Z. Yu, J.L. Luo, and X. Mao","cited_year":"1999","cited_title":"Transgranular stress corrosion cracking of X-80 and X-52 pipeline steels in dilute aqueous solution with near-neutral pH. Corrosion 55(3), 312-318","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560630,"raw_reference":"Gu, B., V. Sizov, L. Yang, and X. Mao. 1999b. Mechanistic studies on non-classical stress corrosion cracking initiation and propagation of pipeline steels in near neutral pH bicarbonate solution. Proc. NACE Northern Region Western Conference (NACE","cited_authors":"Gu, B., V. Sizov, L. Yang, and X. Mao","cited_year":"1999b","cited_title":"Mechanistic studies on non-classical stress corrosion cracking initiation and propagation of pipeline steels in near neutral pH bicarbonate solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560631,"raw_reference":"International, Houston, TX). Harle, B.A. and J.A. Beavers. 1993. Low-pH stress corrosion crack propagation in API X-65 line pipe steel. Corrosion 49, 861-863.","cited_authors":"International, Houston, TX). Harle, B.A. and J.A. Beavers","cited_year":"1993","cited_title":"Low-pH stress corrosion crack propagation in API X-65 line pipe steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560632,"raw_reference":"Harle, B.A., J.A. Beavers, and C.E. Jaske. 1994. Low-pH stress corrosion cracking of natural gas pipelines. Proc. CORROSION/94, NACE International (Houston, TX), paper no. 242.","cited_authors":"Harle, B.A., J.A. Beavers, and C.E. Jaske","cited_year":"1994","cited_title":"Low-pH stress corrosion cracking of natural gas pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560633,"raw_reference":"Harle, B.A., J.A. Beavers, and C.E. Jaske. 1995. Mechanical and metallurgical effects on lowpH stress corrosion cracking of natural gas pipelines. Proc. CORROSION/95, NACE International (Houston, TX), paper no. 646. - A-234 He, D., W. Chen, J. Luo, F. King, T. Jack, and K. Krist. 2000. Effect of surface scratch roughness and orientation on the development of SCC of line pipe steel in near neutral pH environment. Proc. 3rd International Pipeline Conference (ASME, New York, NY), Vol. 2, 997-1004.","cited_authors":"Harle, B.A., J.A. Beavers, and C.E. Jaske","cited_year":"1995","cited_title":"Mechanical and metallurgical effects on lowpH stress corrosion cracking of natural gas pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560634,"raw_reference":"He, D.X., W. Chen, and J.L. Luo. 2004. Effect of cathodic potential on hydrogen content in a pipeline steel exposed to NS4 near-neutral pH soil solution. Corrosion 60(8), 778-786.","cited_authors":"He, D.X., W. Chen, and J.L. Luo","cited_year":"2004","cited_title":"Effect of cathodic potential on hydrogen content in a pipeline steel exposed to NS4 near-neutral pH soil solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560635,"raw_reference":"Holtam, C.M., D.P. Baxter, I.A. Ashcroft, and R.C. Thomson. 2010. Effect of crack depth on fatigue crack growth rates for a C-Mn pipeline steel in a sour environment. Int. J. Fatigue 32, 288-296.","cited_authors":"Holtam, C.M., D.P. Baxter, I.A. Ashcroft, and R.C. Thomson","cited_year":"2010","cited_title":"Effect of crack depth on fatigue crack growth rates for a C-Mn pipeline steel in a sour environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560636,"raw_reference":"Jack, T., M. Wilmott, and W. Chen. 1999. Evaluation of SCC susceptibility of X-70 steel in contact with various soil solutions at near neutral pH: comparison of laboratory predictions with field predictions. Proc. 12th Biennial Joint Research Meeting on Pipeline","cited_authors":"Jack, T., M. Wilmott, and W. Chen","cited_year":"1999","cited_title":"Evaluation of SCC susceptibility of X-70 steel in contact with various soil solutions at near neutral pH: comparison of laboratory predictions with field predictions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560637,"raw_reference":"Research, (Groningen, The Netherlands, May 17-21, 1999), Paper no. 11.","cited_authors":"Research, (Groningen, The Netherlands, May 17-21","cited_year":"1999","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560638,"raw_reference":"Jack, T.R., B. Erno, K. Krist, and R.R. Fessler. 2000. Generation of near neutral pH and high pH SCC environments on buried pipelines. Proc. CORROSION/2000, NACE International (Houston, TX), paper no. 00362.","cited_authors":"Jack, T.R., B. Erno, K. Krist, and R.R. Fessler","cited_year":"2000","cited_title":"Generation of near neutral pH and high pH SCC environments on buried pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560639,"raw_reference":"Jack, T., L. Stehmeier, L. Yang, Y. Cheng, K. Ikeda-Cameron, and R. Muwanga. 2004. Correlation of soil conditions and SCC initiation phenomena to microbial induced corrosion. Gas Research Institute Report, GRI-04/0160.","cited_authors":"Jack, T., L. Stehmeier, L. Yang, Y. Cheng, K. Ikeda-Cameron, and R. Muwanga","cited_year":"2004","cited_title":"Correlation of soil conditions and SCC initiation phenomena to microbial induced corrosion","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560640,"raw_reference":"Johnson, J.T., C.L. Durr, J.A. Beavers, and B.S. Delanty. 2000. Effects of O2 and CO2 on nearneutral-pH stress corrosion crack propagation. Proc. CORROSION/2000, NACE International (Houston, TX), paper no. 00356.","cited_authors":"Johnson, J.T., C.L. Durr, J.A. Beavers, and B.S. Delanty","cited_year":"2000","cited_title":"Effects of O2 and CO2 on nearneutral-pH stress corrosion crack propagation","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560641,"raw_reference":"King, F. and M. Piazza. 2009. Development of guidelines for the identification of SCC sites and the prediction of re-inspection intervals for SCC DA. Proc. CORROSION/2009, NACE International (Houston, TX), paper no. 09111.","cited_authors":"King, F. and M. Piazza","cited_year":"2009","cited_title":"Development of guidelines for the identification of SCC sites and the prediction of re-inspection intervals for SCC DA. Proc","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560642,"raw_reference":"King, F., T. Jack, W. Chen, M. Wilmott, R.R. Fessler, and K. Krist. 2000. Mechanistic studies of initiation and early-stage crack growth for near-neutral pH SCC on pipelines. Proc.","cited_authors":"King, F., T. Jack, W. Chen, M. Wilmott, R.R. Fessler, and K. Krist","cited_year":"2000","cited_title":"Mechanistic studies of initiation and early-stage crack growth for near-neutral pH SCC on pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560643,"raw_reference":"CORROSION/2000, NACE International (Houston, TX), paper no. 00361.","cited_authors":null,"cited_year":null,"cited_title":"CORROSION/2000, NACE International (Houston, TX), paper no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560644,"raw_reference":"Dusek. 2001. Development of a predictive model for the initiation and early-stage growth of near-neutral pH SCC of pipeline steels. Proc. CORROSION/2001, NACE International (Houston, TX), paper no. 01214.","cited_authors":"Dusek","cited_year":"2001","cited_title":"Development of a predictive model for the initiation and early-stage growth of near-neutral pH SCC of pipeline steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560645,"raw_reference":"King, F., G. Van Boven, T.R. Jack, R. Sutherby, and L. Fenyvesi. 2003. Predicting the growth of low- and high-pH SCC on gas transmission pipelines based on operating conditions. In Proc. CORROSION/2003 Research Topical Symposium: Modeling and Prediction of Lifetimes for Corrodible Structures, J.R. Scully and D.W. Shoesmith (eds.), NACE International (Houston, TX), pp. 127-155.","cited_authors":"King, F., G. Van Boven, T.R. Jack, R. Sutherby, and L. Fenyvesi","cited_year":"2003","cited_title":"Predicting the growth of low- and high-pH SCC on gas transmission pipelines based on operating conditions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560646,"raw_reference":"King, F., T. Jack, and L. Yang. 2004. Assessment of the aggressiveness of various types of soil towards low-pH SCC. Gas Research Institute Report, GRI-04/0097. - A-235 King, F., T. Jack, M. Kolar, and R. Worthingham. 2004. A permeable coating model for predicting the environment at the pipe surface under CP-compatible coatings. Proc. 5th International Pipeline Conference (ASME, New York, NY), paper IPC04-0368.","cited_authors":"King, F., T. Jack, and L. Yang","cited_year":"2004","cited_title":"Assessment of the aggressiveness of various types of soil towards low-pH SCC. Gas Research Institute Report, GRI-04/0097","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560647,"raw_reference":"King, F., K. Ikeda-Cameron, T. Jack, and J. Been. 2004b. Long-term environmental monitoring of near-neutral and high-pH SCC sites and the basis of an improved SCC site selection model. Gas Research Institute Report, GRI-04/0098.","cited_authors":"King, F., K. Ikeda-Cameron, T. Jack, and J. Been","cited_year":"2004b","cited_title":"Long-term environmental monitoring of near-neutral and high-pH SCC sites and the basis of an improved SCC site selection model","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560648,"raw_reference":"King, F., T. Jack, M. Kolar, and R. Worthingham. 2004. A permeable coating model for predicting the environment at the pipe surface under CP-compatible coatings. Proc.","cited_authors":"King, F., T. Jack, M. Kolar, and R. Worthingham","cited_year":"2004","cited_title":"A permeable coating model for predicting the environment at the pipe surface under CP-compatible coatings","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560649,"raw_reference":"CORROSION/2004, NACE International (Houston, TX), paper no. 04158.","cited_authors":null,"cited_year":null,"cited_title":"CORROSION/2004, NACE International (Houston, TX), paper no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560650,"raw_reference":"Kuniya, J., H. Anzai, and I. Masaoka. 1992. Effect of MnS inclusions on stress corrosion cracking in low-alloy steels. Corrosion 48(4), 419-425.","cited_authors":"Kuniya, J., H. Anzai, and I. Masaoka","cited_year":"1992","cited_title":"Effect of MnS inclusions on stress corrosion cracking in low-alloy steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560651,"raw_reference":"Kushida, T., K. Nose, H. Asahi, M. Kimura, Y. Yamane, S. Endo, and H. Kawano. 2001. Effects of metallurgical factors and test conditions on near neutral pH SCC of pipeline steels. Proc. CORROSION/2001 (NACE International, Houston, TX), paper no. 01213.","cited_authors":"Kushida, T., K. Nose, H. Asahi, M. Kimura, Y. Yamane, S. Endo, and H. Kawano","cited_year":"2001","cited_title":"Effects of metallurgical factors and test conditions on near neutral pH SCC of pipeline steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560652,"raw_reference":"Lambert, S.B., A. Plumtree, and R. Sutherby. 2000a.. Modeling of environmental crack growth in pipeline steel. Proc. CORROSION/2000, NACE International (Houston, TX), paper no. 00364.","cited_authors":"Lambert, S.B., A. Plumtree, and R. Sutherby","cited_year":"2000a","cited_title":"Modeling of environmental crack growth in pipeline steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560653,"raw_reference":"Lambert, S.B., J.A. Beavers, B. Delanty, R. Sutherby, and A. Plumtree. 2000. Mechanical factors affecting stress corrosion crack growth rates in buried pipelines. Proc. IPC 2000 (ASME, New York, NY), Vol. 2, pp. 961-965. Le Friant, D., B. Bayle, C. Adam, and Th. Magnin. 2000. Stress corrosion cracking of pipeline steels in simulated ground water: from mechanisms to a ranking test. Proc.","cited_authors":"Lambert, S.B., J.A. Beavers, B. Delanty, R. Sutherby, and A. Plumtree","cited_year":"2000","cited_title":"Mechanical factors affecting stress corrosion crack growth rates in buried pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560654,"raw_reference":"EUROCORR 2000, 10-14 September, 2000, London, UK (Institute of Metals, London,","cited_authors":"EUROCORR","cited_year":"2000","cited_title":"10-14 September, 2000, London, UK (Institute of Metals, London","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560655,"raw_reference":"UK). Leis, B.N. 1997. Validation of a high pH stress-corrosion cracking life prediction model (SCCLPM) for gas-transmission pipelines. Report to Line Pipe Research Supervisory","cited_authors":"UK). Leis, B.N","cited_year":"1997","cited_title":"Validation of a high pH stress-corrosion cracking life prediction model (SCCLPM) for gas-transmission pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560656,"raw_reference":"Committee, Program PR 3-9531. Leis, B.N. 1997. Characterization of axial flaws in pipelines, with a focus on stress corrosion cracking. Report to the Line Pipe Research Supervisory Committee, NG-18 Report No. 212, PRCI Catalog No. L51807.","cited_authors":"Committee, Program PR 3-9531. Leis, B.N","cited_year":"1997","cited_title":"Characterization of axial flaws in pipelines, with a focus on stress corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560657,"raw_reference":"Leis, B.N. and W.J. Walsh. 1990. A mechanics-based analysis of stress-corrosion cracking of line-pipe steel in a carbonate-bicarbonate environment. Environmentally Assisted Cracking: Science and Engineering, ASTM STP 1049, W.B. Lisagor, T.W. Crooker, and B.N. Leis (eds.), American Society for Testing and Materials (Philadelphia, PA), pp. 243265.","cited_authors":"Leis, B.N. and W.J. Walsh","cited_year":"1990","cited_title":"A mechanics-based analysis of stress-corrosion cracking of line-pipe steel in a carbonate-bicarbonate environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"journal_article","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560658,"raw_reference":"Leis, B.N. and R.N. Parkins. 1993. Modelling stress-corrosion cracking of high-pressure gas pipelines. In 8th Symposium on Line Pipe Research, American Gas Association Catalog No. L51680, paper no. 19. - A-236 Leis, B.N. and J.A. Colwell. 1997. Initiation of stress-corrosion cracking on gas transmission piping. Effects of the Environment on the Initiation of Crack Growth, ASTM STP 1298, W.A. Van Der Sluys, R.S. Piascik, R. Zawierucha (eds.), American Society for Testing and Materials (Philadelphia, PA), pp. 34-58.","cited_authors":"Leis, B.N. and R.N. Parkins","cited_year":"1993","cited_title":"Modelling stress-corrosion cracking of high-pressure gas pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560659,"raw_reference":"Leis, B.N. and R.N. Parkins. 1998. Mechanics and material aspects in predicting serviceability limited by stress-corrosion cracking. Fatigue Fract. Eng. Materials Struct., 21, 583-601.","cited_authors":"Leis, B.N. and R.N. Parkins","cited_year":"1998","cited_title":"Mechanics and material aspects in predicting serviceability limited by stress-corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560660,"raw_reference":"Leis, B.N., T.P. Forte, and N.D. Ghadiali. 1995. Stress Corrosion Cracking Life Predcition Model – SCCLPM Version 1.0 user's manual and software. Report to Line Pipe Research Supervisory Committee, NG-18 Report No. 217.","cited_authors":"Leis, B.N., T.P. Forte, and N.D. Ghadiali","cited_year":"1995","cited_title":"Stress Corrosion Cracking Life Predcition Model – SCCLPM Version 1.0 user's manual and software","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560661,"raw_reference":"Leis, B.N., J.A. Colwell, T.J. Kilinski, and B. Hindin. 2001. Cyclic stress-behavior and SCC susceptibility of line pipe steels. Report prepared for the Materials Technical Committee, Pipeline Research Council International, Catalog No. L51838.","cited_authors":"Leis, B.N., J.A. Colwell, T.J. Kilinski, and B. Hindin","cited_year":"2001","cited_title":"Cyclic stress-behavior and SCC susceptibility of line pipe steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560662,"raw_reference":"Liu, Z.Y., X.G. Li, C.W. Du, and Y.F. Cheng. 2009. Local additional potential model for effect of strain rate on SCC of pipeline steel in an acidic soli solution. Corrosion Science doi:10.1016/j.corsci.2009.08.019.","cited_authors":"Liu, Z.Y., X.G. Li, C.W. Du, and Y.F. Cheng","cited_year":"2009","cited_title":"Local additional potential model for effect of strain rate on SCC of pipeline steel in an acidic soli solution","cited_venue":null,"cited_doi":"10.1016/j.corsci.2009.08.019","cited_url":null,"ref_kind":"journal_article","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560663,"raw_reference":"Liu, Z.Y., X.G. Li, C.W. Du, L. Lu. Y.R. Zhang, and Y.F. Cheng. 2009. Effect of inclusion on initiation of stress corrosion cracks in X70 pipeline steel in an acidic soil environment. Corrosion Science 51, 895-900.","cited_authors":"Liu, Z.Y., X.G. Li, C.W. Du, L. Lu. Y.R. Zhang, and Y.F. Cheng","cited_year":"2009","cited_title":"Effect of inclusion on initiation of stress corrosion cracks in X70 pipeline steel in an acidic soil environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"journal_article","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560664,"raw_reference":"Liu, Z.Y., X.G. Li, C.W. Du, L.X. Wang, and Y.Z. Huang. 2010. Effect of dissolved oxygen on stress corrosion cracking of X70 pipeline steel in near-neutral pH solution. Corrosion 66, 015006-1 to 015006-6.","cited_authors":"Liu, Z.Y., X.G. Li, C.W. Du, L.X. Wang, and Y.Z. Huang","cited_year":"2010","cited_title":"Effect of dissolved oxygen on stress corrosion cracking of X70 pipeline steel in near-neutral pH solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560665,"raw_reference":"Lu, B.T. and J.L. Luo. 2008. A mechanistic study on near-neutral pH stress corrosion cracking of pipeline steel. Proc. Environmentally Assisted Cracking of Materials. Volume 2:","cited_authors":"Lu, B.T. and J.L. Luo","cited_year":"2008","cited_title":"A mechanistic study on near-neutral pH stress corrosion cracking of pipeline steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560666,"raw_reference":"Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 243-253.","cited_authors":"Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam","cited_year":"2008","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560667,"raw_reference":"Mao, X.X., J.L. Luo, B. Gu, and W. Yu. 1998. Hydrogen facilitated anodic dissolution type stress corrosion cracking of pipeline steels in coating disbondment chemistry. Proc. 2nd International Pipeline Conference (ASME, New York, NY), Vol. I, pp. 485-492.","cited_authors":"Mao, X.X., J.L. Luo, B. Gu, and W. Yu","cited_year":"1998","cited_title":"Hydrogen facilitated anodic dissolution type stress corrosion cracking of pipeline steels in coating disbondment chemistry","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560668,"raw_reference":"Mitsui, H., R. Takahashi, H. Asano, N. Taniguchi, and M. Yui. 2008. Susceptibility to stress corrosion cracking for low-carbon steel welds in carbonate-bicarbonate solution. Corrosion 64, 939-948.","cited_authors":"Mitsui, H., R. Takahashi, H. Asano, N. Taniguchi, and M. Yui","cited_year":"2008","cited_title":"Susceptibility to stress corrosion cracking for low-carbon steel welds in carbonate-bicarbonate solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560669,"raw_reference":"Odziemkowski, M., J. Flis, and D.E. Irish. 1994. Raman spectral and electrochemical studies of surface film formation on iron and its alloys with carbon in Na2CO3/NaHCO3 solution with reference to stress corrosion cracking. Electrochim. Acta, 39, 2225-2236.","cited_authors":"Odziemkowski, M., J. Flis, and D.E. Irish","cited_year":"1994","cited_title":"Raman spectral and electrochemical studies of surface film formation on iron and its alloys with carbon in Na2CO3/NaHCO3 solution with reference to stress corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560670,"raw_reference":"Park, J.J., S.I. Pyun, K.H. Na, S. M. Lee, and Y.T. Kho. 2002. Effect of passivity of the oxide film on low-pH stress corrosion cracking of API 5L X-65 pipeline steel in bicarbonate solution. Corrosion 58(4), 329-336.","cited_authors":"Park, J.J., S.I. Pyun, K.H. Na, S. M. Lee, and Y.T. Kho","cited_year":"2002","cited_title":"Effect of passivity of the oxide film on low-pH stress corrosion cracking of API 5L X-65 pipeline steel in bicarbonate solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560671,"raw_reference":"Parkins, R.N. 1980. Predictive approaches to stress corrosion cracking failure. Corros. Sci. 20, 147-166. - A-237 -","cited_authors":"Parkins, R.N","cited_year":"1980","cited_title":"Predictive approaches to stress corrosion cracking failure","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560672,"raw_reference":"Parkins, R.N. 1989. The application of stress corrosion crack growth kinetics to predicting lifetimes of structures. Corros. Sci. 29, 1019-1038.","cited_authors":"Parkins, R.N","cited_year":"1989","cited_title":"The application of stress corrosion crack growth kinetics to predicting lifetimes of structures","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560673,"raw_reference":"Parkins, R.N. 1992. Environment sensitive cracking of high-pressure pipelines in contact with carbon dioxide-containing solutions. Topical report to Line Pipe Research Supervisory Committee of the American Gas Association, NG-18 Report no. 205 (draft).","cited_authors":"Parkins, R.N","cited_year":"1992","cited_title":"Environment sensitive cracking of high-pressure pipelines in contact with carbon dioxide-containing solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560674,"raw_reference":"PR-232-9401 (draft). Parkins, R.N. 1996. Stress corrosion cracking of pipelines – its control or prevention. Proc.","cited_authors":"PR-232-9401 (draft). Parkins, R.N","cited_year":"1996","cited_title":"Stress corrosion cracking of pipelines – its control or prevention","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560675,"raw_reference":"Parkins, R.N. 1996. Conceptual understanding and life prediction for SCC of pipelines. Proc. Life Prediction of Structures Subject to Environmental Degradation, Research Topical","cited_authors":"Parkins, R.N","cited_year":"1996","cited_title":"Conceptual understanding and life prediction for SCC of pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560676,"raw_reference":"Parkins, R.N. 1998. The influence of hydrogen on crack growth in pipelines. Proc. Materials for Resource Recovery and Transport, L. Collins (ed.), (Metallurgical Society of Canadian Institute of Mining, Metallurgy and Petroleum (CIM), Montreal, QC), p. 35-49.","cited_authors":"Parkins, R.N","cited_year":"1998","cited_title":"The influence of hydrogen on crack growth in pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560677,"raw_reference":"Parkins, R.N. 1998. Effects of hydrogen on low pH stress corrosion crack growth. Report to Line Pipe Research Supervisory Committee of the American Gas Association, final report, PR-232-9704.","cited_authors":"Parkins, R.N","cited_year":"1998","cited_title":"Effects of hydrogen on low pH stress corrosion crack growth","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560678,"raw_reference":"Parkins, R.N. 1999. The involvement of hydrogen in low pH stress corrosion cracking of pipeline steels. Proc. 12th Biennial Joint Research Meeting on Pipeline Research,","cited_authors":"Parkins, R.N","cited_year":"1999","cited_title":"The involvement of hydrogen in low pH stress corrosion cracking of pipeline steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560679,"raw_reference":"Groningen, The Netherlands, May 17-21, 1999, paper no. 10.","cited_authors":"Groningen, The Netherlands, May 17-21","cited_year":"1999","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560680,"raw_reference":"Parkins, R.N. 1999. A review of stress corrosion cracking of pipelines in contact with nearneutral (low) pH solutions. Report to Line Pipe Research Supervisory Committee of the American Gas Association, PR-232-9701.","cited_authors":"Parkins, R.N","cited_year":"1999","cited_title":"A review of stress corrosion cracking of pipelines in contact with nearneutral (low) pH solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560681,"raw_reference":"Parkins, R.N. and R.R. Fessler. 1978. Stress corrosion cracking of high-pressure gas transmission pipelines. Materials in Engineering Applications 1, 80-96.","cited_authors":"Parkins, R.N. and R.R. Fessler","cited_year":"1978","cited_title":"Stress corrosion cracking of high-pressure gas transmission pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560682,"raw_reference":"Parkins, R.N. and R.R. Fessler. 1986. Line pipe stress corrosion cracking – mechanisms and remedies. Proc. CORROSION/86, NACE International (Houston, TX), paper no. 320.","cited_authors":"Parkins, R.N. and R.R. Fessler","cited_year":"1986","cited_title":"Line pipe stress corrosion cracking – mechanisms and remedies","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560683,"raw_reference":"Parkins, R.N. and P.M. Singh. 1990. Stress corrosion crack coalescence. Corrosion 46, 485499.","cited_authors":"Parkins, R.N. and P.M. Singh","cited_year":"1990","cited_title":"Stress corrosion crack coalescence","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560684,"raw_reference":"Parkins, R.N. and B.S. Delanty. 1996. The initiation and early stages of growth of stress corrosion cracks in pipeline steel exposed to a dilute, near-neutral pH solution. Proc. 9th Linepipe Symposium, Pipeline Research Council International, Catalog No. L51746, paper 19.","cited_authors":"Parkins, R.N. and B.S. Delanty","cited_year":"1996","cited_title":"The initiation and early stages of growth of stress corrosion cracks in pipeline steel exposed to a dilute, near-neutral pH solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560685,"raw_reference":"Parkins, R.N. and S. Zhou. 1997. The stress corrosion cracking of C-Mn steel in CO2-HCO3— CO32- solutions. I: Stress corrosion data. Corros. Sci. 39, 159-173. - A-238 -","cited_authors":"Parkins, R.N. and S. Zhou","cited_year":"1997","cited_title":"The stress corrosion cracking of C-Mn steel in CO2-HCO3— CO32- solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560686,"raw_reference":"Parkins, R.N. and S. Zhou. 1997. The stress corrosion cracking of C-Mn steel in CO2-HCO3— CO32- solutions. II: Electrochemical and other data. Corros. Sci. 39, 175-191.","cited_authors":"Parkins, R.N. and S. Zhou","cited_year":"1997","cited_title":"The stress corrosion cracking of C-Mn steel in CO2-HCO3— CO32- solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560687,"raw_reference":"Parkins, R.N. and J.A. Beavers. 2003. Some effects of strain rate on the transgranular stress corrosion cracking of ferritic steels in dilute near-neutral-pH solutions. Corrosion 59(3), 258-273.","cited_authors":"Parkins, R.N. and J.A. Beavers","cited_year":"2003","cited_title":"Some effects of strain rate on the transgranular stress corrosion cracking of ferritic steels in dilute near-neutral-pH solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560688,"raw_reference":"Parkins, R.N., E. Belhimer, and W.K. Blanchard, Jr. 1993. Stress corrosion cracking characteristics of a range of pipeline steels in carbonate-bicarbonate solution. Corrosion 49, 951-966.","cited_authors":"Parkins, R.N., E. Belhimer, and W.K. Blanchard, Jr","cited_year":"1993","cited_title":"Stress corrosion cracking characteristics of a range of pipeline steels in carbonate-bicarbonate solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560689,"raw_reference":"Parkins, R.N., W.K. Blanchard Jr., and B.S. Delanty. 1994. Transgranular stress corrosion cracking of high-pressure pipelines in contact with solutions of near neutral pH. Corrosion 50(5), 394-408.","cited_authors":"Parkins, R.N., W.K. Blanchard Jr., and B.S. Delanty","cited_year":"1994","cited_title":"Transgranular stress corrosion cracking of high-pressure pipelines in contact with solutions of near neutral pH. Corrosion 50(5), 394-408","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560690,"raw_reference":"Pilkey, A.K., S.B. Lambert, and A. Plumtree. 1995. Stress corrosion cracking of X-60 line pipe steel in a carbonate-bicarbonate solution. Corrosion 51, 91-96.","cited_authors":"Pilkey, A.K., S.B. Lambert, and A. Plumtree","cited_year":"1995","cited_title":"Stress corrosion cracking of X-60 line pipe steel in a carbonate-bicarbonate solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560691,"raw_reference":"Plumtree, A., B.W. Williams, S.B. Lambert, and R. Sutherby. 2008. SCC growth in pipeline steel. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H. Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 199-210.","cited_authors":"Plumtree, A., B.W. Williams, S.B. Lambert, and R. Sutherby","cited_year":"2008","cited_title":"SCC growth in pipeline steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560692,"raw_reference":"Psaila-Dombrowski, M.J., A. Van Der Sluys, and B.P. Miglin. 1997. Investigation of pipeline stress corrosion cracking under controlled chemistry conditions. Gas Research Institute","cited_authors":"Psaila-Dombrowski, M.J., A. Van Der Sluys, and B.P. Miglin","cited_year":"1997","cited_title":"Investigation of pipeline stress corrosion cracking under controlled chemistry conditions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560693,"raw_reference":"Report, GRI-97/0001. Puiggali, M., S. Rousserie, and M. Touzet. 2002. Fatigue crack initiation on low-carbon steel pipes in a near-neutral-pH environment under potential control conditions. Corrosion 58(11), 961-970.","cited_authors":"Report, GRI-97/0001. Puiggali, M., S. Rousserie, and M. Touzet","cited_year":"2002","cited_title":"Fatigue crack initiation on low-carbon steel pipes in a near-neutral-pH environment under potential control conditions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560694,"raw_reference":"Qiao, L. and X. Mao. 1995. Thermodynamic analysis on the role of hydrogen in anodic stress corrosion cracking. Acta metal. mater. 43(11), 4001-4006.","cited_authors":"Qiao, L. and X. Mao","cited_year":"1995","cited_title":"Thermodynamic analysis on the role of hydrogen in anodic stress corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560695,"raw_reference":"Qiao, L.J., J.L. Luo, and X. Mao. 1998. Hydrogen evolution and enrichment around stress corrosion crack tips of pipeline steels in dilute bicarbonate solution. Corrosion 54(2), 115-120.","cited_authors":"Qiao, L.J., J.L. Luo, and X. Mao","cited_year":"1998","cited_title":"Hydrogen evolution and enrichment around stress corrosion crack tips of pipeline steels in dilute bicarbonate solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560696,"raw_reference":"Qiao, L.J., J.L. Luo, and X. Mao. 1997. The role of hydrogen in the process of stress corrosion cracking of pipeline steels in dilute carbonate-bicarbonate solution. J. Mater. Sci. Lett. 16, 516-520.","cited_authors":"Qiao, L.J., J.L. Luo, and X. Mao","cited_year":"1997","cited_title":"The role of hydrogen in the process of stress corrosion cracking of pipeline steels in dilute carbonate-bicarbonate solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560697,"raw_reference":"Qin, Z., B. Demko, J. Noël, D. Shoemsith, F. King, R. Worthingham, and K. Keith. 2004. Localized dissolution of millscale-covered pipeline steel surfaces. Corrosion 60, 906914.","cited_authors":"Qin, Z., B. Demko, J. Noël, D. Shoemsith, F. King, R. Worthingham, and K. Keith","cited_year":"2004","cited_title":"Localized dissolution of millscale-covered pipeline steel surfaces","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560698,"raw_reference":"Rebak, R.B., Z. Xia, R. Safruddin, and Z. Szklarska-Smialowska. 1995. Electrochemical processes controlling SCC of underground pipelines. Proc. CORROSION/95, NACE International (Houston, TX), paper no. 184. - A-239 Ramsingh, R.R. and R.W. Revie. 2000. Conditions that lead to the generation of SCC environments. Report for the Corrosion Supervisotry Committee of PRCI, contract PR230-9914, draft report.","cited_authors":"Rebak, R.B., Z. Xia, R. Safruddin, and Z. Szklarska-Smialowska","cited_year":"1995","cited_title":"Electrochemical processes controlling SCC of underground pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560699,"raw_reference":"Rebak, R.B., Z. Xia, R. Safruddin, and Z. Szklarska-Smialowska. 1996. Effect of solution composition and electrochemical potential on stress corrosion cracking of X-52 pipeline steel. Corrosion 52(5), 396-405.","cited_authors":"Rebak, R.B., Z. Xia, R. Safruddin, and Z. Szklarska-Smialowska","cited_year":"1996","cited_title":"Effect of solution composition and electrochemical potential on stress corrosion cracking of X-52 pipeline steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560700,"raw_reference":"Revie, R.W., W. Zheng, F.A. MacLeod, and D. Kiff. 1995. Methodology for realistic full-scale testing of linepipe for stress-corrosion cracking. Pipeline Technology, Vol. I, R. Denys (ed.), Elsevier (Amsterdam), pp. 571-576.","cited_authors":"Revie, R.W., W. Zheng, F.A. MacLeod, and D. Kiff","cited_year":"1995","cited_title":"Methodology for realistic full-scale testing of linepipe for stress-corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560701,"raw_reference":"Senigallia, E. and M. Pontremoli. 1999. Test methodologies for the study of near neutral stress corrosion cracking in pipeline steels (EPRG). Proc. 12th Biennial Joint Research Meeting on Pipeline Research, Groningen, The Netherlands, May 17-21, 1999.","cited_authors":"Senigallia, E. and M. Pontremoli","cited_year":"1999","cited_title":"Test methodologies for the study of near neutral stress corrosion cracking in pipeline steels (EPRG)","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560702,"raw_reference":"Sloterdijk, W. 1996. Chances for high-pH SCC in Gasunie's transmission system. Proc. 9th Linepipe Symposium, Pipeline Research Council International, Catalog No. L51746, paper 18.","cited_authors":"Sloterdijk, W","cited_year":"1996","cited_title":"Chances for high-pH SCC in Gasunie's transmission system","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560703,"raw_reference":"Sutherby, R. and W. Chen. 2004. Deflected stress corrosion cracks in the pipeline steel. Proc.","cited_authors":"Sutherby, R. and W. Chen","cited_year":"2004","cited_title":"Deflected stress corrosion cracks in the pipeline steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560704,"raw_reference":"International Pipeline Conf. 2004 (ASME International, New York, NY), paper IPC040600.","cited_authors":null,"cited_year":null,"cited_title":"International Pipeline Conf","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560705,"raw_reference":"Sutherby, R., T. Jack, G. Van Boven, and M. Wilmott. 2000. CEPA study on characterization of pipeline pressure fluctuations in terms relevant to stress corrosion cracking. Proc. 3rd International Pipeline Conference (ASME, New York, NY), Vol. 2, pp. 989-996.","cited_authors":"Sutherby, R., T. Jack, G. Van Boven, and M. Wilmott","cited_year":"2000","cited_title":"CEPA study on characterization of pipeline pressure fluctuations in terms relevant to stress corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560706,"raw_reference":"Szklarska-Smialowska, Z., Z. Xia, and R.B. Rebak. 1994. Stress corrosion cracking of X-52 carbon steel in dilute aqueous solutions. Corrosion 50(5), 334-338.","cited_authors":"Szklarska-Smialowska, Z., Z. Xia, and R.B. Rebak","cited_year":"1994","cited_title":"Stress corrosion cracking of X-52 carbon steel in dilute aqueous solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560707,"raw_reference":"Tang, X. and Y.F. Cheng. 2009. Micro-electrochemical characterization of the effect of applied stress on local anodic dissolution behavior of pipeline steel under near-neutral ph condition. Electrochim. Acta 54, 1499-1505.","cited_authors":"Tang, X. and Y.F. Cheng","cited_year":"2009","cited_title":"Micro-electrochemical characterization of the effect of applied stress on local anodic dissolution behavior of pipeline steel under near-neutral ph condition","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560708,"raw_reference":"Torres-Islas, A., V.M. Salinas-Bravo, J.L. Albarran, and J.C. Gonzalez-Rodriguez. 2005. Effect of hydrogen on the mechanical properties of X-70 pipeline steel in diluted NaHCO3 solutions at different heat treatments. Int. J. Hydrogen Energy 30, 1317-1322.","cited_authors":"Torres-Islas, A., V.M. Salinas-Bravo, J.L. Albarran, and J.C. Gonzalez-Rodriguez","cited_year":"2005","cited_title":"Effect of hydrogen on the mechanical properties of X-70 pipeline steel in diluted NaHCO3 solutions at different heat treatments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560709,"raw_reference":"Torres-Islas, A., J.G. Gonzalez-Rodriguez, J. Uruchurtu, and S. Serna. 2008. Stress corrosion cracking study of microalloyed pipeline steels in dilute NaHCO3 solutions. Corros. Sci. 50, 2831-2839.","cited_authors":"Torres-Islas, A., J.G. Gonzalez-Rodriguez, J. Uruchurtu, and S. Serna","cited_year":"2008","cited_title":"Stress corrosion cracking study of microalloyed pipeline steels in dilute NaHCO3 solutions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560710,"raw_reference":"Touzet, M., N. Lopez, and M. Puiggali. 1998. Effect of applied potential on cracking of lowalloyed pipeline steel in low pH soil environment. Proc. EUROCORR'98, European Federation of Corrosion, paper no. 226. Van Boven, G., R. Sutherby, and F. King. 2002. Characterizing pressure fluctuations on buried pipelines in terms relevant to stress corrosion cracking. Proc. 4th International Pipeline Conference (ASME, New York, NY), paper IPC2002-27149. - A-240 Van Boven, G., T.R. Jack, and F.King. 2004. Environmental factors: effect on SCC growth. Gas Research Institute Report, GRI-04/0161. Van Boven, G., R. Rogge, and W. Chen. 2006. Residual stress and stress corrosion cracking of high pressure hydrocarbon transmission pipelines. Proc. IPC 2006, ASME (New","cited_authors":"Touzet, M., N. Lopez, and M. Puiggali","cited_year":"1998","cited_title":"Effect of applied potential on cracking of lowalloyed pipeline steel in low pH soil environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560711,"raw_reference":"York, NY), paper IPC2006-10486. Van Boven, G., W. Chen, and R. Rogge. 2007a. The role of residual stress in neutral pH stress corrosion cracking of pipeline steels. Part I: pitting and cracking occurrence. Acta Mater. 55, 29-42. Van Der Sluys, W.A. and R.H. Emanuelson. 1990. Environmental acceleration of fatigue crack growth in reactor pressure vessel materials and environments. Environmentally Assisted Cracking: Science and Engineering, ASTM STP 1049, W.B. Lisagor, T.W.","cited_authors":"York, NY), paper IPC2006-10486. Van Boven, G., W. Chen, and R. Rogge","cited_year":"2007a","cited_title":"The role of residual stress in neutral pH stress corrosion cracking of pipeline steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"journal_article","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560712,"raw_reference":"PA), pp. 117-135. Van Der Sluys, W.A., M. Wilmott, and K. Krist. 1998. Effect of sulfide on stress corrosion crack growth in gas transmission pipe lines. Proc. 2nd International Pipeline Conference (ASME, New York, NY).","cited_authors":"PA), pp. 117-135. Van Der Sluys, W.A., M. Wilmott, and K. Krist","cited_year":"1998","cited_title":"Effect of sulfide on stress corrosion crack growth in gas transmission pipe lines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560713,"raw_reference":"Wang, S-H., W. Chen, T. Jack, F. King, R.R. Fessler, and K. Krist. 2000. Role of prior cyclic loading in the initiation of stress-corrosion cracks on pipeline steels exposed to nearneutral pH environment. Proc. International Pipeline Conf. 2000 (ASME International, New York, NY), vol. 2, pps. 1005-1011.","cited_authors":"Wang, S-H., W. Chen, T. Jack, F. King, R.R. Fessler, and K. Krist","cited_year":"2000","cited_title":"Role of prior cyclic loading in the initiation of stress-corrosion cracks on pipeline steels exposed to nearneutral pH environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560714,"raw_reference":"Wang, S-H., W. Chen, F. King, T.R. Jack, and R.R. Fessler. 2002. Precyclic-loading-induced stress corrosion cracking of pipeline steels in a near-neutral-pH soil environment. Corrosion 58, 526-534.","cited_authors":"Wang, S-H., W. Chen, F. King, T.R. Jack, and R.R. Fessler","cited_year":"2002","cited_title":"Precyclic-loading-induced stress corrosion cracking of pipeline steels in a near-neutral-pH soil environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560715,"raw_reference":"Wang, Y.Z., R.W. Revie, M.T. Shehata, and R.N. Parkins. 1998. Early stages of stress corrosion crack development of X-65 pipeline steel in near-neutral pH solution. Proc. Materials for Resource Recovery and Transport, L. Collins (ed.), (Metallurgical Society of Canadian Institute of Mining, Metallurgy and Petroleum (CIM), Montreal, QC), p. 71-93.","cited_authors":"Wang, Y.Z., R.W. Revie, M.T. Shehata, and R.N. Parkins","cited_year":"1998","cited_title":"Early stages of stress corrosion crack development of X-65 pipeline steel in near-neutral pH solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560716,"raw_reference":"Wang, Y.Z., R.W. Revie, M.T. Shehata, R.N. Parkins, and K. Krist. 1998. Initiation of environment induced cracking in pipeline steel: microstructural correlations. Proc.","cited_authors":"Wang, Y.Z., R.W. Revie, M.T. Shehata, R.N. Parkins, and K. Krist","cited_year":"1998","cited_title":"Initiation of environment induced cracking in pipeline steel: microstructural correlations","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560717,"raw_reference":"International Pipeline Conf. 1998 (ASME International, New York, NY), vol. 1, pps. 529542.","cited_authors":null,"cited_year":null,"cited_title":"International Pipeline Conf","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560718,"raw_reference":"Wang, Y.Z., R.W. Revie, and R.N. Parkins. 1999. Mechanistic aspects of stress corrosion crack initiation and early propagation. Proc. CORROSION/99, NACE International (Houston, TX), paper no. 143.","cited_authors":"Wang, Y.Z., R.W. Revie, and R.N. Parkins","cited_year":"1999","cited_title":"Mechanistic aspects of stress corrosion crack initiation and early propagation","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560719,"raw_reference":"Wang, Z.F. and A. Atrens. 1996. Initiation of stress corrosion cracking for pipeline steels in a carbonate-bicarbonate solution. Met. Mater. Trans. A, 27A, 2686-2691.","cited_authors":"Wang, Z.F. and A. Atrens","cited_year":"1996","cited_title":"Initiation of stress corrosion cracking for pipeline steels in a carbonate-bicarbonate solution","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560720,"raw_reference":"Watson, M.K., M.J. Wilmott, and B. Erno. 1996. Stress corrosion cracking under field simulated conditions. Part II: development of a crack tip model for stress corrosion cracking in carbon dioxide-rich near-neutral pH bulk solutions. Gas Research Institute Report, GRI96/0452.2. - A-241 -","cited_authors":"Watson, M.K., M.J. Wilmott, and B. Erno","cited_year":"1996","cited_title":"Stress corrosion cracking under field simulated conditions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560721,"raw_reference":"Williams, B.W., S.B. Lambert, X.Y. Zhang, A. Plumtree, and R. Sutherby. 2003. Microstructural features of environmentally assisted cracking in pipeline steel. Proc. Environmental Degradation of Materials & Corrosion Control in Metals (EDMCCM), 42nd Annual Conference of Metallurgists of CIM, Vancouver, BC, Canada, J. Luo, M. Elboujdaini, D.","cited_authors":"Williams, B.W., S.B. Lambert, X.Y. Zhang, A. Plumtree, and R. Sutherby","cited_year":"2003","cited_title":"Microstructural features of environmentally assisted cracking in pipeline steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560722,"raw_reference":"Williams, B.W., S.B. Lambert, A. Plumtree, and R. Sutherby. 2004. Environmental crack growth under variable amplitude loading of pipeline steel. Corrosion 60(1), 95-103.","cited_authors":"Williams, B.W., S.B. Lambert, A. Plumtree, and R. Sutherby","cited_year":"2004","cited_title":"Environmental crack growth under variable amplitude loading of pipeline steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560723,"raw_reference":"Wilmott, M.J. and R.L. Sutherby. 1998. The role of pressure and pressure fluctuations in the growth of stress corrosion cracks in line pipe steel. Proc. 2nd International Pipeline Conference (ASME, New York, NY), Vol. 1, 409-421.","cited_authors":"Wilmott, M.J. and R.L. Sutherby","cited_year":"1998","cited_title":"The role of pressure and pressure fluctuations in the growth of stress corrosion cracks in line pipe steel","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560724,"raw_reference":"Wilmott, M.J., T.R. Jack, G. Van Boven, and R.L. Sutherby. 1996. Pipeline stress corrosion cracking: crack growth sensitivity studies under simulated field conditions. Proc.","cited_authors":"Wilmott, M.J., T.R. Jack, G. Van Boven, and R.L. Sutherby","cited_year":"1996","cited_title":"Pipeline stress corrosion cracking: crack growth sensitivity studies under simulated field conditions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560725,"raw_reference":"Wilmott, M.J., G. Van Boven, and T. Jack. 1996. Stress corrosion cracking under field simulated conditions. Part I: electrochemical studies of buried stress corrosion cracking environments. Gas Research Institute Report, GRI-96/0452.1.","cited_authors":"Wilmott, M.J., G. Van Boven, and T. Jack","cited_year":"1996","cited_title":"Stress corrosion cracking under field simulated conditions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560726,"raw_reference":"Yamaguchi, Y., H. Nonaka, and Y. Nishikawa. 1998. Critical cathodic potential and fatigue lifetime evaluation for hydrogen stress cracking on gas transmission pipelines. Proc. 1998 Int. Gas Research Conf., San Diego, CA, pp. 394-404.","cited_authors":"Yamaguchi, Y., H. Nonaka, and Y. Nishikawa","cited_year":"1998","cited_title":"Critical cathodic potential and fatigue lifetime evaluation for hydrogen stress cracking on gas transmission pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560727,"raw_reference":"Youzwishen, O.O., A. Van Aelst, P.F. Ehlers, and A. Nettel. 2004. A statistical model for the prediction of SCC formation along a pipeline. Proc. IPC 2004 (ASME, New York, NY), paper IPC04-0267.","cited_authors":"Youzwishen, O.O., A. Van Aelst, P.F. Ehlers, and A. Nettel","cited_year":"2004","cited_title":"A statistical model for the prediction of SCC formation along a pipeline","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560728,"raw_reference":"Yunovich, M., Z. Xia, and Z. Szklarska-Smialowska. 1998. Factors influencing stress corrosion cracking of carbon steel in diluted bicarbonate environments. Corrosion 54(2), 155-161.","cited_authors":"Yunovich, M., Z. Xia, and Z. Szklarska-Smialowska","cited_year":"1998","cited_title":"Factors influencing stress corrosion cracking of carbon steel in diluted bicarbonate environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560729,"raw_reference":"Zhang, B., J. Fan, Y. Gogotsi, and A. Chudnovsky. 2000. Theoretical and experimental study of stress corrosion cracking of pipeline steel in near neutral pH environment. Proc. 3rd International Pipeline Conference (ASME, New York, NY), Vol. 2, 1013-1020.","cited_authors":"Zhang, B., J. Fan, Y. Gogotsi, and A. Chudnovsky","cited_year":"2000","cited_title":"Theoretical and experimental study of stress corrosion cracking of pipeline steel in near neutral pH environment","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560730,"raw_reference":"Zhang, X.Y., S.B. Lambert, R. Sutherby, and A. Plumtree. 1999. Transgranular stress corrosion cracking of X-60 pipeline steel in simulated ground water. Corrosion 55(3), 297-305.","cited_authors":"Zhang, X.Y., S.B. Lambert, R. Sutherby, and A. Plumtree","cited_year":"1999","cited_title":"Transgranular stress corrosion cracking of X-60 pipeline steel in simulated ground water","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560731,"raw_reference":"Zheng, W., R.W. Revie, F.A. MacLeod, D. Kiff, and S. Rajan. 1995. Testing methods for lowpH pipeline SCC: a comparison of SSRT and full-scale testing. Proc. CORROSION/95,","cited_authors":"Zheng, W., R.W. Revie, F.A. MacLeod, D. Kiff, and S. Rajan","cited_year":"1995","cited_title":"Testing methods for lowpH pipeline SCC: a comparison of SSRT and full-scale testing","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560732,"raw_reference":"Zheng, W., R.W. Revie, O. Dinardo, F.A. MacLeod, W.R. Tyson, and D. Kiff. 1996. Pipeline","cited_authors":"Zheng, W., R.W. Revie, O. Dinardo, F.A. MacLeod, W.R. Tyson, and D. Kiff","cited_year":"1996","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560733,"raw_reference":"SCC in near-neutral pH environment: effects of environmental and metallurgical variables. Proc. 9th Linepipe Symposium, Pipeline Research Council International, Catalog No. L51746, paper 22. - A-242 Zheng, W., R.W. Revie, W.R. Tyson, G. Shen, F.A. MacLeod, and D. Kiff. 1996. Pipeline SCC in near-neutral pH environment: results of full-scale tests. Proc. CORROSION/96,","cited_authors":"SCC in near-neutral pH environment: effects of environmental and metallurgical variables. Proc. 9th Linepipe Symposium, Pipeline Research Council International, Catalog No. L51746, paper 22. - A-242 Zheng, W., R.W. Revie, W.R. Tyson, G. Shen, F.A. MacLeod, and D. Kiff","cited_year":"1996","cited_title":"Pipeline SCC in near-neutral pH environment: results of full-scale tests","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560734,"raw_reference":"Zheng, W., F.A. MacLeod, R.W. Revie, W.R. Tyson, G. Shen, D. Kiff, M. Skaff, and E-W. Wong. 1997. Recent progress in the study of transgranular SCC in line pipe steels. Proc. 2nd International Conference on Corrosion-Deformation Interactions-CDI '96 (European Federation of Corrosion Report No. 21), paper 28, pp. 282-292.","cited_authors":"Zheng, W., F.A. MacLeod, R.W. Revie, W.R. Tyson, G. Shen, D. Kiff, M. Skaff, and E-W. Wong","cited_year":"1997","cited_title":"Recent progress in the study of transgranular SCC in line pipe steels","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560735,"raw_reference":"Zheng, W., R.W. Revie, F.A. MacLeod, O. Dinardo, D. Kiff, andJ. McKinnon. 1998. Low pH","cited_authors":"Zheng, W., R.W. Revie, F.A. MacLeod, O. Dinardo, D. Kiff, andJ. McKinnon","cited_year":"1998","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560736,"raw_reference":"Zheng, W., R. Sutherby, R.W. Revie, W.R. Tyson, and G. Shen. 2000. Stress corrosion cracking of linepipe steels in near-neutral pH environment: a review of the effects of stress. In ASTM Special Technical Publication, STP 1401, Environmentally Assisted Cracking Predictive Methods for Risk Assessment and Evaluation of Materials, Equipment and Structures, R.D. Kane (ed.), American Society for Testing and Materials (West Conshohocken, PA), pp. 473-483.","cited_authors":"Zheng, W., R. Sutherby, R.W. Revie, W.R. Tyson, and G. Shen","cited_year":"2000","cited_title":"Stress corrosion cracking of linepipe steels in near-neutral pH environment: a review of the effects of stress","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560737,"raw_reference":"Zhigletsova, S.K., V.B. Rodin, V.V. Rudavin, G.E. Rasulova, N.A. Alexandrova, G.M. Polomina, and V.P. Kholodenko. 2008. Change of physiochemical parameters of soils near stress-corrosion defects on gas pipelines. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H. Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 323333. - B-1 -","cited_authors":"Zhigletsova, S.K., V.B. Rodin, V.V. Rudavin, G.E. Rasulova, N.A. Alexandrova, G.M. Polomina, and V.P. Kholodenko","cited_year":"2008","cited_title":"Change of physiochemical parameters of soils near stress-corrosion defects on gas pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560738,"raw_reference":"IGSCC observed in pure sulphate solutions at pH 8 Yunovich et al. (1998)","cited_authors":"IGSCC observed in pure sulphate solutions at pH 8 Yunovich et al","cited_year":"1998","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560739,"raw_reference":"IGSCC observed at (cathodic) potentials at which dissolution could not be involved. Contrary to suggestions of a dissolution mechanism for IG cracking Crack path seems dependent on pH with IGSCC prevalent at higher pH. Possible evidence for a transition in crack path from TG to IG with increasing pH. Increasing temperature results in higher crack growth rates and a wider potential window for cracking. The activation energy for high-pH SCC cracks is of the order of 42 kJ/mol. Application of CP current density ca polarize a mill-scaled or rusted steel surface into the cracking range. In lab tests, a cathodic current density of 60 µA/cm2 was sufficient to polarize the surface into the cracking range. iR drop along the disbondment can shift the potential into the cracking range. Thus, the complete loss of CP may not be necessary to shift the potential into the cracking range. The required environment could be generated by CP elsewhere in the disbondment and diffuse to the location of permissible potential. Associated SCC Guideline Yunovich et al. (1998) Yunovich et al. (1998) SzklarskaSmialowska et al. (1994) SzklarskaSmialowska et al. (1994) SzklarskaSmialowska et al. (1994)","cited_authors":"IGSCC observed at (cathodic) potentials at which dissolution could not be involved. Contrary to suggestions of a dissolution mechanism for IG cracking Crack path seems dependent on pH with IGSCC prevalent at higher pH. Possible evidence for a transition in crack path from TG to IG with increasing pH. Increasing temperature results in higher crack growth rates and a wider potential window for cracking. The activation energy for high-pH SCC cracks is of the order of 42 kJ/mol. Application of CP current density ca polarize a mill-scaled or rusted steel surface into the cracking range. In lab tests, a cathodic current density of 60 µA/cm2 was sufficient to polarize the surface into the cracking range. iR drop along the disbondment can shift the potential into the cracking range. Thus, the complete loss of CP may not be necessary to shift the potential into the cracking range. The required environment could be generated by CP elsewhere in the disbondment and diffuse to the location of permissible potential. Associated SCC Guideline Yunovich et al","cited_year":"1998","cited_title":"Yunovich et al","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560740,"raw_reference":"H-0-6 Parkins (1996) H-0-2, H-I-1, H-IV-2 Parkins (1996) H-I-4, H-I-15 Parkins (1996) H-I-4 continued ….. - B-3 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no. H010 H011 H012 H013 H014 H015 R&D Guideline Overprotection at potentials more negative than -1.1 VSCE can result in H2 bubbles that block CP and shift potential into cracking range. Another mechanism by","cited_authors":"H-0-6 Parkins","cited_year":"1996","cited_title":"H-0-2, H-I-1, H-IV-2 Parkins (1996) H-I-4, H-I-15 Parkins (1996) H-I-4 continued ….. - B-3 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560741,"raw_reference":"SCC failures have been observed for steels with a wide range of chemical composition. Reference Associated SCC Guideline Jack et al. (2000) H-I-2 Sutherby and Chen (2004) Sutherby and Chen (2004) Odziemkowski et al. (1994)","cited_authors":"SCC failures have been observed for steels with a wide range of chemical composition. Reference Associated SCC Guideline Jack et al","cited_year":"2000","cited_title":"H-I-2 Sutherby and Chen (2004) Sutherby and Chen (2004) Odziemkowski et al","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560742,"raw_reference":"H-I-7 Parkins (1994) H-I-13 continued ….. - B-6 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no. H029 H030 H031 H032 H033 H034 H035 H036 R&D Guideline Lifetime prediction requires a stochastic approach. Scatter observed in coating failure, crack initiation (which is associated with pitting), crack growth, resulting in a distribution of apparent crack growth rates, which must be treated statistically. High-pH SCC is uncommon on liquid pipelines. Because of the lower temperature generally associated with liquid lines, although there have been vases in warm climates (Saudi Arabia), and the shipment of hot liquids could induce this form of cracking. High-pH SCC cracks follow an intergranular path. This implies a fundamental weakness at grain boundaries, thought to be associated with the cyclic stress-strain behaviour. Field evidence for Fe3O4 with some FeCO3 on fracture surfaces. These observations are consistent with lab findings (see H025) No evidence for role of stress raisers for high-pH SCC. Unlike NNpH SCC for which stress raisers are very important, there is no indication that stress raisers are necessary for high-pH SCC, although cracking has been observed in dents. Probably appropriate to state that stress raisers are not","cited_authors":"H-I-7 Parkins","cited_year":"1994","cited_title":"H-I-13 continued ….. - B-6 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560743,"raw_reference":"H-III-4 H-II-5 H-II-2 Parkins (1994)","cited_authors":"H-III-4 H-II-5 H-II-2 Parkins","cited_year":"1994","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560744,"raw_reference":"IGSCC is observed over a wide range of pH (pH 6.6-11). Why is high-pH SCC only reported in the range ~pH 9.5-11.5? Is the potential never in the right region? Peak crack growth rate shifts to more-negative potentials with increasing T. On the assumption that more-negative potentials are more likely because of the effects of CP, then high-pH is more likely at higher T. Francis and Jandu (2006)","cited_authors":"IGSCC is observed over a wide range of pH (pH 6.6-11). Why is high-pH SCC only reported in the range ~pH 9.5-11.5? Is the potential never in the right region? Peak crack growth rate shifts to more-negative potentials with increasing T. On the assumption that more-negative potentials are more likely because of the effects of CP, then high-pH is more likely at higher T. Francis and Jandu","cited_year":"2006","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560745,"raw_reference":"H-III-3 Parkins (1996) H-0-5 Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) Parkins and Zhou (1997a) Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) H-IV-2 continued ….. - B-18 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no. H141 H142 H143 H144 H145 H146 H147 H148 H149 H150 R&D Guideline","cited_authors":"H-III-3 Parkins","cited_year":"1996","cited_title":"H-0-5 Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) Parkins and Zhou (1997a) Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) H-0-6 Parkins and Zhou (1997a) H-IV-2 continued ….. - B-18 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560746,"raw_reference":"SCC crack patterns observed, including the effect of coalescence. Implies no role for effects due to dissolution of inclusions, development of local chemistry, electrochemical effects of millscale, … Once dormant, cracks in a dense patch will remain dormant. I.e., a dense crack patch cannot become a sparse dense patch! Reference Associated SCC Guideline Parkins and Zhou (1997a) H-IV-4 Parkins and Zhou (1997b) Parkins and Zhou (1997b) H-0-6 Parkins and Zhou (1997b)","cited_authors":"SCC crack patterns observed, including the effect of coalescence. Implies no role for effects due to dissolution of inclusions, development of local chemistry, electrochemical effects of millscale, … Once dormant, cracks in a dense patch will remain dormant. I.e., a dense crack patch cannot become a sparse dense patch! Reference Associated SCC Guideline Parkins and Zhou","cited_year":"1997a","cited_title":"H-IV-4 Parkins and Zhou (1997b) Parkins and Zhou (1997b) H-0-6 Parkins and Zhou (1997b)","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560747,"raw_reference":"Leis (1997) H-III-3 continued ….. - B-19 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no. H151 H152 H153 H154 H155 H156 H157 H158 H159 H160 H161 R&D Guideline Microstructure has effect on crack path. Cracks propagate according to microstructure, tending to prefer propagating along gb, especially in coarsergrained material. Weld metal is less susceptible to high-pH SCC than base metal. Thought to be due to finer grain structure of weld metal. Cracks avoid pearlite or pearlite-dispersed regions. Consistent with suggestion elsewhere that cracks could arrest at pearlite grain boundaries. Mild cyclic loading (R = 0.9) enhances crack initiation by reducing threshold stress. Reported by others, but confirmed here for low stress range Threshold stress lower on as-received (millscale) surface. Although the magnitude of the difference here was not great. Density of cracks increases with increasing load. Implication is that more cracks likely with higher loads, but that the cracks will be denser (and,","cited_authors":"Leis","cited_year":"1997","cited_title":"H-III-3 continued ….. - B-19 Table B.1: R&D Guidelines – High-pH SCC (continued) Ref no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560748,"raw_reference":"SCC and readily permeates in C-steel and can be concentrated by residual and applied stress is consistent with a role of H in NNpH SCC. Reference Associated SCC Guideline Gu et al. (1999) N-0-7 Gu et al. (1999) N-0-7 Gu et al. (1999) Been et al. (2006) N-I-9, N-IV-1 Been et al. (2006) N-I-9, N-IV-1 Been et al. (2006) N-I-10, N-IV-1, N-IV-2 Qiao and Mao (1998) Qiao et al. (1997)","cited_authors":"SCC and readily permeates in C-steel and can be concentrated by residual and applied stress is consistent with a role of H in NNpH SCC. Reference Associated SCC Guideline Gu et al","cited_year":"1999","cited_title":"N-0-7 Gu et al","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560749,"raw_reference":"N-III-1 Parkins (1998) N-0-9 continued …. - B-26 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N014 N015 N016 N017 N018 N019 N020 R&D Guideline Susceptibility to SCC increases in the presence of CO2. %RA tends to decrease with increasing CO2, although much scatter. At pH 5.8, %RA decreases monotonically with decreasing pH, but at pH 6.5 and pH 8 minimum ductility at around ECORR with second loss of ductility at more-negative potentials (possibly associated with HIC). Proposed role of CO2 is to lower pH to promote H evolution. No systematic effect of temperature. No systematic dependence of %RA on temperature between 5oC and 45oC. Evidence for role of H in NNpH SCC. Cracking occurs at potentials below H equilibrium line, presence of quasi-cleavage on fracture surface characteristic of","cited_authors":"N-III-1 Parkins","cited_year":"1998","cited_title":"N-0-9 continued …. - B-26 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560750,"raw_reference":"HIC, rather than NNpH SCC, is the predominant process for cathodically polarized samples. Similar %RA at -1.0 VSCE regardless of presence of CO2 or not Rebak et al. (1996) Associated SCC Guideline Brousseau and Qian (1994) Asher and Singh (2009) N-II-6 Asher and Singh (2009) N-II-1 Asher and Singh (2009) N-0-9 Been et al. (2006) N-0-10, N-IV-2, N-IV-4 Been et al. (2006) Gu et al. (1999) N-0-4 Gu et al. (1999) Gu et al. (1999) N-0-7 continued …. - B-29 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N042 N043 N044 N045 N046 N047 N048 N049 R&D Guideline Threshold S content of 0.01-0.02 wt.% for the susceptibility of reactor pressure vessel steels to corrosion fatigue. Similarities between this system and NNpH SCC of pipeline steels proposed by Gabetta (1997). Eadie et al. (2005) proposed important role of S in NNpH SCC environments. Question is whether a similar threshold value exists for NNpH SCC. Hydrogen threshold for HSC/HIC is 10 ppb. If correct, then many of the NNpH SCC studies based on a correlation between H content may, in fact, be related to HSC rather than NNpH SCC. There should exist a potential threshold between NNpH SCC and HSC/HIC. And that threshold, the source of which is a threshold H content, will depend on the nature of the environment (e.g., pH, presence of H-recombination poisons, etc.) Corrosion fatigue mechanism under severe loading conditions. da/dN = C(K)m, for R = 0.5 and 0.82 at 40 cycles/day and R = 0.9 at 5000 cycles/day","cited_authors":"HIC, rather than NNpH SCC, is the predominant process for cathodically polarized samples. Similar %RA at -1.0 VSCE regardless of presence of CO2 or not Rebak et al","cited_year":"1996","cited_title":"Associated SCC Guideline Brousseau and Qian (1994) Asher and Singh (2009) N-II-6 Asher and Singh (2009) N-II-1 Asher and Singh (2009) N-0-9 Been et al","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560751,"raw_reference":"TG cracking. Reference Associated SCC Guideline Beavers and Jaske (2004) N-0-10, N-III-4, N-III-5, N-IV-4 Beavers and Jaske (2004) N-0-10, N-III-4, N-III-5, N-IV-4 Beavers and Jaske (2004) Beavers and Jaske (2004) Beavers and Jaske (2004) N-0-10, N-IV-3 Beavers and Jaske (2004) N-0-10, N-IV-2, N-IV-4 Gangloff (1985)","cited_authors":"TG cracking. Reference Associated SCC Guideline Beavers and Jaske","cited_year":"2004","cited_title":"N-0-10, N-III-4, N-III-5, N-IV-4 Beavers and Jaske (2004) N-0-10, N-III-4, N-III-5, N-IV-4 Beavers and Jaske (2004) Beavers and Jaske (2004) Beavers and Jaske (2004) N-0-10, N-IV-3 Beavers and Jaske (2004) N-0-10, N-IV-2, N-IV-4 Gangloff (1985)","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560752,"raw_reference":"N-III-6 Gangloff (1985) continued …. - B-39 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N110 N112 N113 N114 N115 N116 N117 N118 R&D Guideline Environmental enhancement due to effects of cyclic loading on crack chemistry and promotion of H absorption for short cracks. Short cracks have high surface area:volume ratios. O2 consumed on crack walls so that crack-tip pH is maintained low and promotes H+ reduction and H absorption. In the case of HSS, acidification due to hydrolysis of Cr(III). Short cracks grow up to a factor of 10 faster than long cracks in sour environments. Results for X-65 pipeline steel and, although a sour environment, of some relevance to NNpH SCC. At a K~9 MPam1/2, transition from short to long cracks occurs at ~6 mm. Accelerated growth of short cracks likely due to environmental effect on H absorption at crack tip. Could be result of lower crack-tip pH for short cracks or, if bulk charging is most important, gradient of [H] across wall thickness. Crack initiation favoured on original pipe surface and at pits or regions of corrosion. Although original pipe surface was not compared with polished surface, more cracks initiated on external vs. internal surface. Cyclic load tests done under","cited_authors":"N-III-6 Gangloff","cited_year":"1985","cited_title":"continued …. - B-39 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560753,"raw_reference":"CGR. Although the cathodic polarization was done ostensibly to simulate the apparent effect of millscale, could simulate any source of cathodic polarization, e.g., partial CP penetration. Dormant cracks can be reactivated by resumption of more-aggressive cyclic loading. Apparent that dormant cracks are just that, they are dormant rather than dead. Apparently relatively easy to reactivate cracks after as long as 4 days without growth. Crack growth is strongly dependent on strain rate. da/dN decreases but da/dt increases with increasing frequency. Reference Associated SCC Guideline He et al. (2000) Eadie et al. (2002) N-I-9 Eadie et al. (2002) Been et al. (2004) N-I-9 Been et al. (2004) N-I-9, N-II-1 Been et al. (2006) N-0-3 Been et al. (2006) N-I-18 Been et al. (2006) N-III-9 Been et al. (2006) N-0-3 continued …. - B-44 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N156 N157 N158 N159 N160 N161 N162 N163 N164 N165 R&D Guideline NNpH SCC crack growth controlling process changes as crack grows. Threeregime \"map' developed, with strain-rate control under mild loading conditions, CF model at intermediate loading conditions, and rapid cracking at high KMAX Under mild loading conditions, a crack-tip strain rate model is appropriate. Based on poor fit of CF model to field data at low KMAX/K, strain rate model deemed to be more appropriate, especially given observation of strain rate dependence of da/dt (da/dt = 0.0085","cited_authors":"CGR. Although the cathodic polarization was done ostensibly to simulate the apparent effect of millscale, could simulate any source of cathodic polarization, e.g., partial CP penetration. Dormant cracks can be reactivated by resumption of more-aggressive cyclic loading. Apparent that dormant cracks are just that, they are dormant rather than dead. Apparently relatively easy to reactivate cracks after as long as 4 days without growth. Crack growth is strongly dependent on strain rate. da/dN decreases but da/dt increases with increasing frequency. Reference Associated SCC Guideline He et al","cited_year":"2000","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560754,"raw_reference":"CGR is correlated with crack-tip strain rate. However, because of variability in models used to predict , cannot use this correlation to predict CGR's on pipelines. Use frequency and R ratio to rank tendency for cracks to become dormant. Can be done based on correlation in guideline N100, but this figure may be specific to crack geometry and the environment. See also N166 Unload-reload transients can increase the CGR and re-initiate dormant cracks. Occurred in majority of lab cases. Overloads had no consistent effect on CGR or dormant cracks. Neither the occurrence nor the magnitude of overloads had a clear effect in the lab. Simulated hydrotests did not affect dormant cracks but slowed active cracks. Hydrotesting does not re-activate dormant cracks, but does slow actively growing cracks (due to introduction of compressive zone ahead of crack). Reference Associated SCC Guideline Been et al. (2006) N-III-3, N-III-5 Been et al. (2006) N-III-3, N-III-5 Been et al. (2006) Been et al. (2006) N-0-10, N-IV-4 Beavers (2004)","cited_authors":"CGR is correlated with crack-tip strain rate. However, because of variability in models used to predict , cannot use this correlation to predict CGR's on pipelines. Use frequency and R ratio to rank tendency for cracks to become dormant. Can be done based on correlation in guideline N100, but this figure may be specific to crack geometry and the environment. See also N166 Unload-reload transients can increase the CGR and re-initiate dormant cracks. Occurred in majority of lab cases. Overloads had no consistent effect on CGR or dormant cracks. Neither the occurrence nor the magnitude of overloads had a clear effect in the lab. Simulated hydrotests did not affect dormant cracks but slowed active cracks. Hydrotesting does not re-activate dormant cracks, but does slow actively growing cracks (due to introduction of compressive zone ahead of crack). Reference Associated SCC Guideline Been et al","cited_year":"2006","cited_title":"N-III-3, N-III-5 Been et al","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560755,"raw_reference":"N-III-3 Beavers (2004) N-III-8, N-III-9 Beavers (2004) N-III-2, N-III-9 Beavers (2004)","cited_authors":"N-III-3 Beavers","cited_year":"2004","cited_title":"N-III-8, N-III-9 Beavers (2004) N-III-2, N-III-9 Beavers (2004)","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560756,"raw_reference":"Beavers (2004) continued …. - B-45 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. R&D Guideline Reference Associated SCC Guideline Beavers (2004) N-III-8, N-III-9 Beavers (2004) N-III-9, N-III-10 A critical crack-tip strain rate exists below which cracks go dormant. The value of the critical crack-tip strain rate is uncertain because of variability in models to","cited_authors":"Beavers","cited_year":"2004","cited_title":"continued …. - B-45 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560757,"raw_reference":"SSRT ductility. There is no single soil extract parameter that correlates with SCC susceptibility. Conclusion is that there is unlikely to be a single parameter that can be used to rank SCC sites. More-negative ECORR (native potential) and redox potential is an indicator of higher susceptibility (as measured by SSRT and H-perm). Suggestion is that native potentials could be used as a measure of susceptibility. Consistent with observation of more-negative redox potentials at field SCC sites. Reference Associated SCC Guideline Beavers (2004) Jack et al. (1999) Zheng et al. (1995) N-II-1 Watson et al. (1996) N-0-9 PsailaDombrowski et al. (1997) N-IV-11 King et al. (2004a) King et al. (2004a) N-I-2 King et al. (2004a) N-I-1 continued …. - B-47 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N176 N177 N178 N179 N180 N181 N182 N183 R&D Guideline","cited_authors":"SSRT ductility. There is no single soil extract parameter that correlates with SCC susceptibility. Conclusion is that there is unlikely to be a single parameter that can be used to rank SCC sites. More-negative ECORR (native potential) and redox potential is an indicator of higher susceptibility (as measured by SSRT and H-perm). Suggestion is that native potentials could be used as a measure of susceptibility. Consistent with observation of more-negative redox potentials at field SCC sites. Reference Associated SCC Guideline Beavers","cited_year":"2004","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560758,"raw_reference":"CP. Based on experimental observation using simulated disbondment and application of CP with and without CO2 purge. Gradation of corrosion damage along disbondment due to potential gradient. Less corrosion near mouth, pitting at intermediate locations, and general corrosion furthest from mouth. Penetration of CP will depend on various factors, including: disbondment height, current density, conductivity of solution, physical/spatial restrictions. Under cyclic loading, pits in disbonded region nucleate cracks. Cracks initiate some distance away from disbondment mouth at location where pits nucleate. Initial surface condition of steel plate unknown. Cyclic loading can induce a burst of room-temperature creep of pipeline steels. Creep burst could have significance for crack initiation and growth for both high-pH and NNpH SCC. Aggressive soils exhibit a narrow range of pH as a function of CO2 partial pressure. May indicate that highly buffered solutions are more aggressive. However, in this study aggressiveness was determined by TTF of SSRT, so question of what is being measured. Reference Associated SCC Guideline Van Boven et al. (2007b)","cited_authors":"CP. Based on experimental observation using simulated disbondment and application of CP with and without CO2 purge. Gradation of corrosion damage along disbondment due to potential gradient. Less corrosion near mouth, pitting at intermediate locations, and general corrosion furthest from mouth. Penetration of CP will depend on various factors, including: disbondment height, current density, conductivity of solution, physical/spatial restrictions. Under cyclic loading, pits in disbonded region nucleate cracks. Cracks initiate some distance away from disbondment mouth at location where pits nucleate. Initial surface condition of steel plate unknown. Cyclic loading can induce a burst of room-temperature creep of pipeline steels. Creep burst could have significance for crack initiation and growth for both high-pH and NNpH SCC. Aggressive soils exhibit a narrow range of pH as a function of CO2 partial pressure. May indicate that highly buffered solutions are more aggressive. However, in this study aggressiveness was determined by TTF of SSRT, so question of what is being measured. Reference Associated SCC Guideline Van Boven et al","cited_year":"2007b","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560759,"raw_reference":"SCC colonies associated with mean maximum sub-surface (0-2 mm) residual stress of 220 MPa. Maximum residual stress corresponds to plateau value observed at depths between ~1-2 mm. No SCC colonies associated with mean maximum sub-surface (0-2 mm) residual stress of 100 MPa. Maximum residual stress corresponds to plateau value observed at depths between ~1-2 mm. Reference Associated SCC Guideline Beavers et al. (2001) Beavers et al. (2001) Beavers et al. (2001) N-I-5 Beavers et al. (2001) Beavers et al. (2001) Beavers et al. (2000) N-I-11, N-III-12 Beavers et al. (2000) N-III-12 Beavers et al. (2000) N-I-11, N-III-12 Beavers et al. (2000) N-I-11 continued …. - B-57 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N254 N255 N256 N257 N258 N259 N260 N261 N262 N263 R&D Guideline Increased microhardness levels show weak correlation with SCC colonies. Evidence for some correlation between increasing microhardness and SCC colonies, but correlation is weak. Rougher surfaces associated with SCC colonies. Increased probability of finding","cited_authors":"SCC colonies associated with mean maximum sub-surface (0-2 mm) residual stress of 220 MPa. Maximum residual stress corresponds to plateau value observed at depths between ~1-2 mm. No SCC colonies associated with mean maximum sub-surface (0-2 mm) residual stress of 100 MPa. Maximum residual stress corresponds to plateau value observed at depths between ~1-2 mm. Reference Associated SCC Guideline Beavers et al","cited_year":"2001","cited_title":"Beavers et al","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560760,"raw_reference":"Parkins (1992) Associated SCC Guideline N-0-4 N-0-2 Parkins (1992)","cited_authors":"Parkins","cited_year":"1992","cited_title":"Associated SCC Guideline N-0-4 N-0-2 Parkins (1992)","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560761,"raw_reference":"N-I-8 Parkins (1999) N-I-8 continued …. - B-63 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no. N311 N312 N313 N314 N315 N316 N317 N318 N319 N320 N321 N322 R&D Guideline Uncertain whether new multilayer coatings will support NNpH SCC. Such coatings may exhibit apparently beneficial effects of FBE and/or the surface prep required to apply FBE or the detrimental effects of tape coating Do Cl- and SO42- play an active role in NNpH SCC? Cracking can be obtained in pure water purged with CO2, yet all trapped waters contain Cl- and sulphate. Crack initiation is not random, but is directed. Cracks often initiate just ahead of existing crack tips, or around periphery of un-corroded area with pit in centre, or adjacent to tape coating. Dormant cracks can be reactivated if they coalesce with growing crack. Static load near yield stress is insufficient to initiate cracks. Pipelines operating","cited_authors":"N-I-8 Parkins","cited_year":"1999","cited_title":"N-I-8 continued …. - B-63 Table B.2: R&D Guidelines – Near-neutral pH SCC (continued) Ref no","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560762,"raw_reference":"SCC. Preliminary study, careful about over-interpreting. Bending stress more important for crack on shoulder on an unconstrained dent than the hoop stress. Implies cracks associated with dents will grow in non-axial orientations Hydrotest procedure will not necessarily slow the subsequent growth of cracks in a dent. Based on CTOD observations of effect of simulation hydrotest on growth in air of crack on shoulder of unconstrained dent. Reference Associated SCC Guideline Parkins (1999)","cited_authors":"SCC. Preliminary study, careful about over-interpreting. Bending stress more important for crack on shoulder on an unconstrained dent than the hoop stress. Implies cracks associated with dents will grow in non-axial orientations Hydrotest procedure will not necessarily slow the subsequent growth of cracks in a dent. Based on CTOD observations of effect of simulation hydrotest on growth in air of crack on shoulder of unconstrained dent. Reference Associated SCC Guideline Parkins","cited_year":"1999","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560763,"raw_reference":"N-III-9 Parkins (1999) N-0-3, N-II-2 Parkins (1999)","cited_authors":"N-III-9 Parkins","cited_year":"1999","cited_title":"N-0-3, N-II-2 Parkins (1999)","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560764,"raw_reference":"N-I-19 Parkins (1999) N-0-9 Davis and Parkins (1992) Brongers et al. (2009) N-I-12 Brongers et al. (2009) continued …. - B-64 -","cited_authors":"N-I-19 Parkins","cited_year":"1999","cited_title":"N-0-9 Davis and Parkins (1992) Brongers et al","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560765,"raw_reference":"SCC, than FBE For shielding coatings, bare area adjacent to disbondment prevents any protection under disbondment. Thus, for PE ctg, a bare area will be preferentially polarised with no CP reaching disbondment. However, bare area has less effect of distribution of current for CTE which is generally permeable. Inadequate grit blasting can lead to no improvement in SCC resistance. Appear to require a white surface finish, rather than near-white, to ensure sufficient grit blasting to prevent SCC. Older FBE lines may have been inadequately blasted. Cracks in dense crack patches tend to become dormant because of shielding by neighbouring cracks. Dense patches defined as those with a crack spacing of <20% of the wall thickness) Cracks in sparse crack patches can continue to grow unhindered by shielding. A crack patch is not the same as a crack colony, the latter being more defined by the shape and size of the disbondment. Complex 3-D interaction of stress within a crack patch with the crack-tip stress increasing, decreasing, or remaining constant with increasing depth under various circumstances. High-pH and NNpH SCC cracks show similar characteristics in terms of crack size, spacing, and shape Reference Associated SCC Guideline Beavers (1992)","cited_authors":"SCC, than FBE For shielding coatings, bare area adjacent to disbondment prevents any protection under disbondment. Thus, for PE ctg, a bare area will be preferentially polarised with no CP reaching disbondment. However, bare area has less effect of distribution of current for CTE which is generally permeable. Inadequate grit blasting can lead to no improvement in SCC resistance. Appear to require a white surface finish, rather than near-white, to ensure sufficient grit blasting to prevent SCC. Older FBE lines may have been inadequately blasted. Cracks in dense crack patches tend to become dormant because of shielding by neighbouring cracks. Dense patches defined as those with a crack spacing of <20% of the wall thickness) Cracks in sparse crack patches can continue to grow unhindered by shielding. A crack patch is not the same as a crack colony, the latter being more defined by the shape and size of the disbondment. Complex 3-D interaction of stress within a crack patch with the crack-tip stress increasing, decreasing, or remaining constant with increasing depth under various circumstances. High-pH and NNpH SCC cracks show similar characteristics in terms of crack size, spacing, and shape Reference Associated SCC Guideline Beavers","cited_year":"1992","cited_title":null,"cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560766,"raw_reference":"Beavers (1992) N-I-8 Leis and Colwell (1997) N-III-8 Leis and Colwell (1997) N-III-14, N-IV-10 Leis and Colwell (1997) Leis and Colwell (1997) continued …. - B-65 -","cited_authors":"Beavers","cited_year":"1992","cited_title":"N-I-8 Leis and Colwell (1997) N-III-8 Leis and Colwell (1997) N-III-14, N-IV-10 Leis and Colwell (1997) Leis and Colwell (1997) continued …. - B-65 -","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560767,"raw_reference":"SCC for cracks away from the failure but show no clear trend with depth for cracks that lead to failure. Hydrogen plays a significant role in NNpH SCC, but the mechanism has not been identified. In a correlative site-selection model for a single pipeline, three parameters were found to be key predictors of NNpH SCC: pipe manufacturer, coating type, and soil type.  >4 times more likely to find SCC in glaciofluvial soil than in lacustrine soil  >3 times more likely to find SCC under asphalt coating compared with other coatings (CTE, epoxy urethane, FBE, tape, wax)  >18 times more likely for pipe from manufacturer G to exhibit SCC than pipe from manufacturers A, B, or C Susceptibility to NNpH SCC increases with decreasing O2 concentration. Dissolution of millscale can lead to axially aligned corrosion pits or trenches which act as ideal crack initiation sites Millscale is electrochemically active and participates in the crack initiation and growth process. Although there is no evidence in support or contrary, millscale may exhibit varying electrochemical activity resulting in varying susceptibility. Van Boven et al. (2002) Castaneda et al. (2008) Associated SCC Guideline N-0-8 Castaneda et al. (2008) Castaneda et al. (2008)","cited_authors":"SCC for cracks away from the failure but show no clear trend with depth for cracks that lead to failure. Hydrogen plays a significant role in NNpH SCC, but the mechanism has not been identified. In a correlative site-selection model for a single pipeline, three parameters were found to be key predictors of NNpH SCC: pipe manufacturer, coating type, and soil type.  >4 times more likely to find SCC in glaciofluvial soil than in lacustrine soil  >3 times more likely to find SCC under asphalt coating compared with other coatings (CTE, epoxy urethane, FBE, tape, wax)  >18 times more likely for pipe from manufacturer G to exhibit SCC than pipe from manufacturers A, B, or C Susceptibility to NNpH SCC increases with decreasing O2 concentration. Dissolution of millscale can lead to axially aligned corrosion pits or trenches which act as ideal crack initiation sites Millscale is electrochemically active and participates in the crack initiation and growth process. Although there is no evidence in support or contrary, millscale may exhibit varying electrochemical activity resulting in varying susceptibility. Van Boven et al","cited_year":"2002","cited_title":"Castaneda et al","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560768,"raw_reference":"ASME. 2004. Integrity Management of Stress Corrosion Cracking in Gas Pipeline High Consequence Areas. ASME Standards Technology Publication STP-PT-011, American Society for Mechanical Engineers (New York, NY).","cited_authors":"ASME","cited_year":"2004","cited_title":"Integrity Management of Stress Corrosion Cracking in Gas Pipeline High Consequence Areas","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560769,"raw_reference":"ASTM. 2005. ASTM Standard E1049-85(2005), Standard Practices for Cycle Counting in Fatigue. ASTM International, West Conshohocken, PA, 2006, DOI: 10.1520/E104985R05.","cited_authors":"ASTM","cited_year":"2005","cited_title":"ASTM Standard E1049-85(2005), Standard Practices for Cycle Counting in Fatigue","cited_venue":null,"cited_doi":"10.1520/e104985r05","cited_url":null,"ref_kind":"journal_article","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560770,"raw_reference":"Baker. 2005. Stress Corrosion Cracking Study. Prepared by Michael Baker Jr., Inc. for the U.S. Department of Transportation, Office of Pipeline Safety. TTO Number 8, Integrity Management Program Delivery Order DTRS56-02-D-70036.","cited_authors":"Baker","cited_year":"2005","cited_title":"Stress Corrosion Cracking Study","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560771,"raw_reference":"Beavers, J.A. and W.V. Harper. 2004. Stress corrosion cracking prediction model. Proc.","cited_authors":"Beavers, J.A. and W.V. Harper","cited_year":"2004","cited_title":"Stress corrosion cracking prediction model","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560772,"raw_reference":"Beavers, J.A. and R.G. Worthingham. 2002. The influence of soil chemistry on SCC of underground pipelines. Proc. 4th International Pipeline Conference (ASME, New York,","cited_authors":"Beavers, J.A. and R.G. Worthingham","cited_year":"2002","cited_title":"The influence of soil chemistry on SCC of underground pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"government_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560773,"raw_reference":"NY), paper IPC2002-27146. Beavers, J.A., J.T. Johnson, and R.L. Sutherby. 2000. Materials factors influencing the initiation of near-neutral pH SCC on underground pipelines. Proc. International Pipeline","cited_authors":"NY), paper IPC2002-27146. Beavers, J.A., J.T. Johnson, and R.L. Sutherby","cited_year":"2000","cited_title":"Materials factors influencing the initiation of near-neutral pH SCC on underground pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560774,"raw_reference":"CEPA. 1998. CEPA Stress Corrosion Cracking Database: First Trending Report. Canadian Energy Pipeline Association (Calgary, AB).","cited_authors":"CEPA","cited_year":"1998","cited_title":"CEPA Stress Corrosion Cracking Database: First Trending Report","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560775,"raw_reference":"CEPA. 2000. CEPA Stress Corrosion Cracking Database: Second Trending Report. Canadian Energy Pipeline Association (Calgary, AB).","cited_authors":"CEPA","cited_year":"2000","cited_title":"CEPA Stress Corrosion Cracking Database: Second Trending Report","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"dataset","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560776,"raw_reference":"King, F., G. Van Boven, T.R. Jack, R. Sutherby, and L. Fenyvesi. 2003. Predicting the growth of low- and high-pH SCC on gas transmission pipelines based on operating conditions. In Proc. CORROSION/2003 Research Topical Symposium: Modeling and Prediction of Lifetimes for Corrodible Structures, J.R. Scully and D.W. Shoesmith (eds.), NACE International (Houston, TX), pp. 127-155. - C-40 King, F., K. Ikeda-Cameron, T. Jack, and J. Been. 2004. Long-term environmental monitoring of near-neutral and high-pH SCC sites and the basis of an improved SCC site selection model. Gas Research Institute Report, GRI-04/0098.","cited_authors":"King, F., G. Van Boven, T.R. Jack, R. Sutherby, and L. Fenyvesi","cited_year":"2003","cited_title":"Predicting the growth of low- and high-pH SCC on gas transmission pipelines based on operating conditions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560777,"raw_reference":"Leeson, R. and D.K. Spitzmacher. 2006. SCC inspection & mitigation program on Suncor","cited_authors":"Leeson, R. and D.K. Spitzmacher","cited_year":"2006","cited_title":"SCC inspection & mitigation program on Suncor","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560778,"raw_reference":"Penner, L., G. Mollard, M. Holm, and R. Sutherby. 2003. Geological, geotechnical and hydrogeological setting of a gas pipeline failure near Brandon, Manitoba. In Proc. 56th Annual Canadian Geotech. Conf., Canadian Geotechnical Society (Ottawa, ON)","cited_authors":"Penner, L., G. Mollard, M. Holm, and R. Sutherby","cited_year":"2003","cited_title":"Geological, geotechnical and hydrogeological setting of a gas pipeline failure near Brandon, Manitoba","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560779,"raw_reference":"Inquiry, NEB Report MH-2-95. National Energy Board (Calgary, AB). Van Boven, G., R. Sutherby, and F. King. 2002. Characterizing pressure fluctuations on buried pipelines in terms relevant to stress corrosion cracking. Proc. 4th International Pipeline Conference (ASME, New York, NY), paper IPC2002-27149. Van Boven, G., T.R. Jack, and F. King. 2004. Environmental factors: effect on SCC growth. Gas Research Institute Report, GRI-04/0161.","cited_authors":"Inquiry, NEB Report MH-2-95. National Energy Board (Calgary, AB). Van Boven, G., R. Sutherby, and F. King","cited_year":"2002","cited_title":"Characterizing pressure fluctuations on buried pipelines in terms relevant to stress corrosion cracking","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560780,"raw_reference":"Wilmott, M.J. and D.A. Diakow. 1996. Factors influencing stress corrosion cracking of gas transmission pipelines: detailed studies following a pipeline failure. Part 1: environmental considerations. Proc. International Pipeline Conference (ASME, New","cited_authors":"Wilmott, M.J. and D.A. Diakow","cited_year":"1996","cited_title":"Factors influencing stress corrosion cracking of gas transmission pipelines: detailed studies following a pipeline failure","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560781,"raw_reference":"York, NY), Vol. 1, pp. 507-524. Youzwishen, O.O., A. Van Aelst, P.F. Ehlers, and A. Nettel. 2004. A statistical model for the prediction of SCC formation along a pipeline. Proc. IPC 2004 (ASME, New York, NY), paper IPC04-0267.","cited_authors":"York, NY), Vol. 1, pp. 507-524. Youzwishen, O.O., A. Van Aelst, P.F. Ehlers, and A. Nettel","cited_year":"2004","cited_title":"A statistical model for the prediction of SCC formation along a pipeline","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560782,"raw_reference":"Zhigletsova, S.K., V.B. Rodin, V.V. Rudavin, G.E. Rasulova, N.A. Alexandrova, G.M. Polomina, and V.P. Kholodenko. 2008. Change of physiochemical parameters of soils near stress-corrosion defects on gas pipelines. Proc. Environmentally Assisted Cracking of Materials. Volume 2: Prediction, Industrial Developments and Evaluation. S.A. Shipilov, R.H. Jones, J.-M. Olive, and R.B. Rebak (eds.), (Elsevier, Amsterdam, 2008), pp. 323333. - D-1 -","cited_authors":"Zhigletsova, S.K., V.B. Rodin, V.V. Rudavin, G.E. Rasulova, N.A. Alexandrova, G.M. Polomina, and V.P. Kholodenko","cited_year":"2008","cited_title":"Change of physiochemical parameters of soils near stress-corrosion defects on gas pipelines","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560783,"raw_reference":"Been, J., F. King, and R. Sutherby. 2008. Environmentally assisted cracking of pipeline steels in near-neutral pH environments. In Proc. Second International Conference on Environment-Induced Cracking of Metals (EICM-2), Banff, AB, September 20-23, 2004 (Elsevier, Amsterdam), Volume 2, p. 221-232.","cited_authors":"Been, J., F. King, and R. Sutherby","cited_year":"2008","cited_title":"Environmentally assisted cracking of pipeline steels in near-neutral pH environments","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560784,"raw_reference":"King, F., G. Van Boven, T. Jack, R. Sutherby, and L. Fenyvesi. 2003. Predicting the growth of low- and high-pH SCC on gas transmission pipelines based on operating conditions. Proc. CORROSION/2003 Research Topical Symposium, NACE International (Houston,","cited_authors":"King, F., G. Van Boven, T. Jack, R. Sutherby, and L. Fenyvesi","cited_year":"2003","cited_title":"Predicting the growth of low- and high-pH SCC on gas transmission pipelines based on operating conditions","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560785,"raw_reference":"TX). King, F., K. Ikeda-Cameron, T. Jack, and J. Been. 2004. Long-term environmental monitoring of near-neutral and high-pH SCC sites and the basis of an improved SCC site selection model. Gas Research Institute Report, GRI-04/0098.","cited_authors":"TX). King, F., K. Ikeda-Cameron, T. Jack, and J. Been","cited_year":"2004","cited_title":"Long-term environmental monitoring of near-neutral and high-pH SCC sites and the basis of an improved SCC site selection model","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560786,"raw_reference":"OSPL pipeline: field data trends and observations. Proc. 6th International Pipeline Conference (ASME, New York, NY), paper IPC2006-10060. Le Friant, D., B. Bayle, C. Adam, and Th. Magnin. 2000. Stress corrosion cracking of pipeline steels in simulated ground water: from mechanisms to a ranking test. Proc. - D-28 EUROCORR 2000, 10-14 September, 2000, London, UK (Institute of Metals, London,","cited_authors":"OSPL pipeline: field data trends and observations. Proc. 6th International Pipeline Conference (ASME, New York, NY), paper IPC2006-10060. Le Friant, D., B. Bayle, C. Adam, and Th. Magnin","cited_year":"2000","cited_title":"Stress corrosion cracking of pipeline steels in simulated ground water: from mechanisms to a ranking test","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560787,"raw_reference":"UK). NEB. 1996. Stress Corrosion Cracking on Canadian Oil and Gas Pipelines, Report of the","cited_authors":"UK). NEB","cited_year":"1996","cited_title":"Stress Corrosion Cracking on Canadian Oil and Gas Pipelines, Report of the","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null},{"citation_id":1560788,"raw_reference":"York, NY), Vol. 1, pp. 507-524. Youzwishen, O.O., A. Van Aelst, P.F. Ehlers, and A. Nettel. 2004. A statistical model for the prediction of SCC formation along a pipeline. Proc. IPC 2004 (ASME, New York, NY), paper IPC04-0267. Research & Development Program Guidelines for the Identification of SCC Sites and the Estimation of Re-Inspection Intervals for SCCDA Main Objective","cited_authors":"York, NY), Vol. 1, pp. 507-524. Youzwishen, O.O., A. Van Aelst, P.F. Ehlers, and A. Nettel","cited_year":"2004","cited_title":"A statistical model for the prediction of SCC formation along a pipeline","cited_venue":null,"cited_doi":null,"cited_url":null,"ref_kind":"research_report","section":"refsec","page":null,"context_sentence":null,"paper_id":null,"paper_title":null,"paper_year":null,"paper_doi":null}]}